Next Article in Journal / Special Issue
Single-Step Synthesis Process for High-Entropy Transition Metal Boride Powders Using Microwave Plasma
Previous Article in Journal / Special Issue
Prediction of Sodium Substitution Sites in Octacalcium Phosphate: The Relationships of Ionic Pair Ratios in Reacting Solutions
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Communication

Synthesis of Oxide Ceramics in Detonating Atmosphere

Laboratoire des Nanomatériaux pour Systèmes Sous Sollicitations Extrêmes (NS3E), ISL-CNRS-UNISTRA UMR 3208, Institut Franco-Allemand de Recherches de Saint-Louis (ISL), 5 Rue du Général Cassagnou, BP70034, 68301 Saint-Louis, France
Submission received: 25 March 2021 / Revised: 17 May 2021 / Accepted: 19 May 2021 / Published: 21 May 2021
(This article belongs to the Special Issue Advances in Ceramics)

Abstract

:
A detonation process based on 2,4,6 trinitrotoluene (TNT), used as an energetic reagent, was successfully implemented in the synthesis of a series of metal oxide ceramics. TNT offers better physicochemical and mechanical properties than the energetic compounds traditionally used in such processes, thus offering safer handling and transport conditions. The experimental procedure, which consisted to of mixing the energetic molecule with a ceramic salt, was simple to perform. The detonation products were characterized by X-ray diffraction, scanning and transmission electron microscopies, energy dispersive X-ray spectroscopy and nitrogen physisorption. The as-synthesized ceramic powders (CeO2, HfO2, Nb2O5, and In2O3) were crystalline and made of nano-sized quasi-spherical particles. This investigation provides an enhanced detonation synthesis process for elaborating ceramics. The majority of the oxide materials mentioned in this study had never previously been prepared by the detonation process.

1. Introduction

An explosion or detonation is a powerful, high-temperature (>1000 °C) decomposition chemical reaction that releases a large amount of heat and pressure (GPa), as well as a large volume of gases, in a few microseconds [1]. Explosives, molecules that detonate, are most of the time used as a destructive source by the military (e.g., bombs, warheads and ammunition) or for civil engineering (e.g., road construction, mining, comminuting, avalanche maintenance, hazardous land stabilization, etc.). High-tech fields such as the exploration of space or in-orbit placement of satellites by means of launchers are also significant consumers of explosives [1].
In the 1960s, explosion or detonation was used to synthesize materials—in particular, sp3-hybridation carbon phases like diamonds (ND) [2]. Nano-sized NDs were, thus, collected in the detonation soot after the detonation of a 2,4,6 trinitrotoluene/1,3,5 trinitro-1,3,5-triazine (TNT/RDX) mixture. Other carbon structures like nanotubes (NTs) were successfully synthesized by explosion from an energetic mixture based on 2,4,6-trinitrophenol (TNP), paraffin and benzene at the beginning of the 2000s [3]. The detonation process was also implemented to create ceramic materials as oxides or, in a few cases, carbide materials [4]. Single (Al2O3, ZrO2, TiO2, etc.) and mixed (LiMn2O4, MnFe2O4, SrAl2O4, etc.) oxides were, thus, synthesized from energetic charges made of RDX or ammonium nitrate (AN, NH4NO3) as detonative compounds mixed with metallic salts as ceramic sources [5,6,7,8,9,10,11,12,13,14,15]. More recently, the TNT molecule was offered as an explosive source to synthesize zirconia nanopowder from polymer-coated zirconium sulfate tetra hydrate, and pure silicon carbide (SiC) nanoparticles were prepared by the detonation of a TNT/RDX energetic charge previously mixed with a preceramic polymer (polycarbosilane) [16,17].
Herein, a series of transition metal oxide ceramics were successfully synthesized by using the detonation process. Trinitrotoluene (TNT), a secondary explosive molecule, was used as the energetic source. Compared to the energetic materials most often used in such an approach, i.e., AN and RDX compounds that exhibit a high chemical sensitivity toward metallic species [18] and higher sensitivities to mechanical stimulus [19], respectively, the TNT molecule can be seen to be a safer alternative and is, therefore, of the highest interest. In addition in the present investigation, the experimental procedure has been significantly revised compared to [16] in order to drastically reduce the number of steps and then make it easier to implement. Two main changes, both highly time-consuming, were thus made, namely the removal of the use of a polymer additive (coated on the surface of the metal salt particles before mixing with the explosive molecule to avoid possible friction phenomena between ceramic and explosive particles during pressing step) and the temperature-controlled hydraulic pressing step which was replaced by a manual encapsulating of the as-prepared energetic mixture in a plastic tube (before detonation experiment). To date, to the best of our knowledge, the synthesis by detonation of HfO2, Nb2O5, and In2O3 ceramics has not been reported. These ceramic oxides, in particular those based on niobium and indium, have been selected for their potential interest as oxidizers in the formulation of metal/oxide ceramic energetic composites (i.e., thermites) [20,21]. Over the last two decades, these energetic materials have attracted increasing attention in pyrotechnics due to the use of nanopowders that significantly improve their intrinsic performance (ease of ignition, increased burning rate, etc.) [22].

2. Materials and Methods

The 2,4,6 trinitrotoluene (TNT, C6H2(NO2)3CH3) explosive molecule was purchased from Eurenco (Sorgues, France). Cerium sulfate tetra hydrate (Ce(SO4)2·4H2O, 98+%), hafnium dichloride oxide octahydrate (HfOCl2·8H2O, 98+%), niobium (V) oxalate hydrate (C10H5NbO20·xH2O, 99%), and indium (III) acetate (In(OOCCH3)3, 99.99%) were obtained from Alfa Aesar (Ward Hill, MA, USA). Heptane (C7H16, reagent grade) was obtained from Prolabo (Paris, France). Chemicals were used without further purification.
The experimental procedure conducted in this investigation was as follows: 225 g of TNT explosive molecule was mixed with 25 g of ceramic salt (90:10 wt. %) in 250 mL of heptane. The suspension was filtrated and the solid phase dried at 70 °C for 12 h. The resulting dry powdered mixture (230–250 g) was placed in a polypropylene tube (Ø = 43 mm, L = 150 mm). A booster (graphite/wax/1,3,5-trinitro-1,3,5-triazinane secondary explosive (RDX), 0.5/5/94.5 wt. %, m = 55 g, Ø = 28.4 mm, L = 57.5 mm) and a non-electric initiator (Titanobel) were added to the tube containing the TNT/ceramic salt mixture, in order to achieve an energetic train (Figure 1A). A booster was placed between the non-electric initiator and the energetic charge to obtain a reliable initiation and propagation of a stable detonation within the TNT/ceramic salt mixture. On the basis of our own experiments, the 90:10 wt. % ratio of explosives and ceramic salts is considered as a good compromise, since a charge richer in ceramic salts produces a larger amount of material but with a larger particle size, whereas a charge richer in explosives synthesizes smaller particles but in greatly reduced quantities. The loading density was about 1.138 g/cm3, 1.098 g/cm3, 1.053 g/cm3 and 1.094 g/cm3, corresponding to a theoretical maximum density (TMD) of 65%, 64.9%, 63.3% and 64.5%, for the TNT/Ce, TNT/Hf, TNT/Nb and TNT/In mixture, respectively. The energetic train was placed in a volume of demineralized water (3 L, cooling medium for detonation products) and placed at the centre of a detonation chamber (Figure 1B) before the reaction took place. The detonation experiments were triggered by connecting the detonation cable of the non-electric initiator to a specific device capable of generating a high-energy, high-temperature spark. Finally, a purification process (filtration, oxidizing heat treatment (650 °C, 30 min) and acid etching (hydrochloric acid 2M)) was performed to collect the as-detonated ceramic material of the detonation soot.
The structure and microstructure of the as-detonated materials were investigated by means of an X-ray diffractometer (XRD, D8 Advance, Bruker, Billerica, MA, USA) and a scanning and transmission electron microscope (SEM-Nova NanoSEM 450 and TEM-CM200, FEI, Hillsboro, OR, USA), respectively. The textural properties (specific surface areas, pore volumes) of the powders, degassed at 200 °C for 6 h, were determined by nitrogen adsorption measurements at 77K (ASAP 2020, Micromeritics, Norcross, GA, USA). Specific surface area (SSA) was determined by taking into account the Brunauer‒Emmett‒Teller (BET) theory in the relative pressure range of p/p0 = 0.05–0.25 and the pore volumes were measured at p/p0 = 0.99.

3. Results

Figure 2 shows the XRD patterns of the different ceramics synthesized by detonation. The diffraction peaks of patterns A to D were attributed to cerium (IV) oxide (CeO2, cubic structure, Fm-3m (225) space group), hafnium (IV) oxide (HfO2, monoclinic structure, P21/a (14) space group), niobium (V) oxide (T-Nb2O5, orthorhombic structure-Pbam space group), and indium (III) oxide (In2O3, cubic structure, Ia-3 (206) space group), respectively. The Miller planes were reported on the corresponding diffraction peaks, taking care to maintain the readability of the patterns. The removal of any amorphous carbon phases was systematically verified by thermo gravimetric analyses (not shown here).
The coherence lengths or crystallite size (L) of oxide materials were determined using the Scherrer Equation (1):
Lhkl = k × λ/(β × cosθhkl)
with k a dimensionless constant (0.89), λ the wavelength of the X-ray radiation (λCu), β the line broadening at full width at half maximum intensity (FWHM, corrected by the instrumental line broadening) and θ the Bragg angle of the considered (h,k,l) Miller plane. Taking into account the most intense diffraction peak, namely the (111), (−111), (001) and (222) peaks for the CeO2, HfO2, Nb2O5 and In2O3 materials, respectively, coherence lengths were determined to be equal to 29 nm, 25 nm, 43 nm and 36 nm for the respective materials.
The microstructure (morphology and size) of the oxide ceramics was examined by scanning electron microscopy (SEM). The ceramic materials consist of micron-sized particles (<1 µm) coated by a plethora of smaller ones (Supplementary Materials). Representative views of this second population of particles (majority in number) are presented on magnified pictures in Figure 3 (top) for CeO2, HfO2, Nb2O5 and In2O3. The particles exhibit a quasi-spherical morphology with a size lower than 50 nm regardless of the material considered. The particle size distributions of the different samples could not be determined by dynamic light scattering measurements because of the polydispersity of the samples (micro- and nano-particles).
Additional characterizations by energy-dispersive X-ray spectroscopy supported the chemical nature of the as-detonated products (all kind of particles) since only the cerium, hafnium, niobium and indium metals and oxygen were identified on the different elemental mappings (Supplementary Materials). Traces of titanium, silicium, aluminum and iron originated from the set-up were also observed on particles bigger than 1 µm. The four oxide materials were characterized by a transmission electron microscopy (TEM) analysis. At low magnifications, the images support the synthesis of oxide powders consisting of both micron (<µm) and nanometer (largely dominant part) particles, as previously observed by SEM technique (Supplementary Materials). Representative images of nanoparticles are shown in Figure 3 (down). The size of these nanoparticles ranges from 20 to 50 nm, which is consistent with what was observed in the previous SEM characterization (<50 nm).
Nitrogen physisorption measurements were performed on the different oxide ceramics synthesized by detonation. The representative isotherms are displayed in Figure 4. According to the IUPAC standard, the four curves exhibit type-IV profiles with H3 hysteresis loops [23].
Taking into account the BET model, specific surface areas of 22, 23, 28, and 20 m²/g were determined for the CeO2, HfO2, Nb2O5, and In2O3 powders, respectively. Assuming dense, monodisperse and spherical particles, regardless of the chemical nature of the powder considered, the main particles’ sizes (Ø) were calculated by means of the Formula (2) [23]:
Ø = 6/(ρ × SSA)
where ρ is the density (7.22, 9.68, 4.60, and 7.18 g/cm3 for CeO2, HfO2, Nb2O5 and In2O3 oxide materials, respectively) and SSA the corresponding specific surface area. Average particle sizes of 37 nm, 27 nm, 46 nm, and 42 nm were, thus, calculated for the cerium, hafnium, niobium, and indium oxides, respectively. These data were consistent with the sizes observed by the SEM analysis for each material, especially for the smallest particles, and thus confirm the high predominance of nano-sized particles (in volume) over micron-sized particles. Pore volumes at p/p0 = 0.99 were determined to be equal to 0.11, 0.10, 0.09, and 0.10 cm3/g for the CeO2, HfO2, Nb2O5, and In2O3 materials, respectively. With respect to the hysteresis loops, characteristics of non-rigid aggregates [23], large mesopores are expected as no plateaus were observed at high relative pressure p/p0. Pore size distributions (PSD), calculated from the Brunauer–Jarrett–Halenda (BJH) model applied to the desorption branches of the nitrogen isotherms, confirmed the existence of pores of large size ranging from 10 to 200 nm and corresponding to inter-particle porosity (Figure 4, insert).

4. Discussion

Based on the chemistry of explosives [24], the mechanism for the reaction taking place during the detonation process can be suggested. Conventionally, the explosive molecule, when it detonates, breaks into the smallest possible entities such as atoms, which then leads to the formation of small stable inert species, for example, nitrogen (N2), water (H2O), carbon mono/di-oxide (CO/CO2), etc. The nature and amount of the species strongly depend on the oxygen available within the explosive molecule considered. For instance, for the 2,4,6 trinitrotoluene molecule, when privileging the Kistiakowsky‒Wilson rules [24], the decomposition reaction will be as follows:
2C7H5N3O6(s) → 3N2(g) + 5H2O(g) + 7CO(g) + 7C(s)
This corroborates the above definition by supplying solid carbon phases since the oxygen present in TNT is not sufficient to completely oxidize the molecule. In fact, the oxygen balance, a factor that allows us to quantity the oxygen available to completely oxidize the considered molecule, is negative for the TNT compound (−77%). Now, considering a mixture of TNT with a ceramic salt (considered inert in the present investigation), the decomposition reaction of TNT will destroy the ceramic molecule and, thus, all atoms coming from the explosive and inert molecules will take part in the formation of detonation products. Accordingly, assuming 1 g of mixture (0.9 TNT/0.1 ceramic salt), the following global decomposition reactions can be offered:
0.00396 C7H5N3O6(s) + 0.00025 Ce(SO4)2·4H2O(s) → 0.00594 N2(g) + 0.0109 H2O(g) + 0.01436 CO(g) +
0.01336 C(s) + 0.00025 CeO2(s) + 0.0005 SO2(g)
0.00396 C7H5N3O6 (s) + 0.00029 HfOCl2·8H2O(s) → 0.00594 N2 (g) + 0.01222 H2O (g) + 0.01357 CO(g) +
0.01415 C(s) + 0.00029 HfO2(s) + 0.00029 Cl2(g)
0.00396 C7H5N3O6 (s) + 0.00015 C10H5NbO20·6H2O(s) → 0.00594 N2(g) + 0.01121 H2O(g) + 0.01617 CO(g) +
0.01305 C(s) + 0.00008 Nb2O5(s)
0.00396 C7H5N3O6 (s) + 0.00034 In(OOCCH3)3(s) → 0.00594 N2(g) + 0.01143 H2O(g) + 0.01386 CO(g) +
0.0159 C(s) + 0.00017 In2O3(s)
In summary, carbon and oxide ceramic (CeO2, HfO2, Nb2O5, and In2O3) solid phases should be produced during the different detonation experiments. This hypothesis is consistent with the data obtained from the characterization techniques for all the detonation experiments above.
With regard to the particle size and shape of ceramic oxides synthesized by the detonation route, it is difficult to make a statement on the influence of just one specific parameter, as the detonation reaction is an extremely complex process involving decomposition, gasification and condensation reactions. However, the high pressures (GPa), the high temperatures (>1000 °C) generated during detonation (µs) and the subsequent cooling rate (109 °C/s) play an undeniable role on the morphology and nanometric dimension of the materials thus prepared [1,2,24]. For example, for nanodiamonds (NDs) synthesized by detonation of highly energetic explosives—and for which similar characteristics in terms of size (nm) and morphology are obtained—a mechanism of condensation of ultra-dispersed phases in a supersaturated gaseous phase combined with a rapid dispersion of the fluid environment (in a cooling medium) is suggested [25,26]. While the former affects the morphology, the latter is a key parameter for controlling the size of the particles produced. It can, therefore, be assumed that a similar mechanism occurs for the oxide materials prepared in the present study. Regarding the micron-sized particles found in all detonation soots, it can be speculated that their formation is due to several parameters such as the configuration of the charge (cylinder) as well as the porosity inside the charge (around 35% assuming a loading density of 65% of the TMD for the different formulations), which can lead to the creation of zones where the generated temperatures and pressures are mitigated compared to the zones at the origin of the nanoparticle formation [5]. Therefore, the quenching of detonation products from these zones is not as drastic to control the growth of nanoscale particles and, therefore, the particles can grow. Another point could be the non-homogeneous dispersion of the ceramic salts in the energetic phase of TNT—creating inert phase micro-domains—which would fuel the growth of particles beyond the nanoscale. Currently, the concept of detonation synthesis, and, more particularly, the experimental parameters, are rethought in order to improve the current results because the fact that nano- and micro-particles coexist can make it difficult to apply additional treatments.

5. Conclusions

Ceramic materials, i.e., cerium (IV) oxide, hafnium (IV) oxide, niobium (V) oxide, and indium (III) oxide, were synthesized by an explosion process. The insensitive 2,4,6 trinitrotoluene (TNT) explosive molecule was, therefore, mixed with a ceramic salt (90:10 wt. %) in a non-polar solvent. After removal of the solvent, the resulting energetic charge was detonated in an aqueous medium to condense the detonation products. The experimental conditions resulted in the elaboration of crystalline ceramic powders with quasi-spherical particles of less 50 nm in size. This was the first report of the synthesis of HfO2, Nb2O5, and In2O3 materials by means of this process. The present approach is expected to generate increasing attention in the preparation and scaling of nanomaterials, although improvements are needed to make such as-detonated samples reliable for a subsequent sintering process.

Supplementary Materials

The following are available online at https://0-www-mdpi-com.brum.beds.ac.uk/article/10.3390/ceramics4020019/s1, Figure S1: SEM (top) and TEM (down) low magnified images of pristine oxide ceramics: (A) CeO2, (B) HfO2, (C) Nb2O5, and (D) In2O3. Figure S2: Elemental mappings of the different calcinated as-detonated oxide ceramics: (A) CeO2, (B) HfO2, (C) Nb2O5, and (D) In2O3. The qualitative analyses were carried out by using a scanning electron microscope (SEM-JEOL JSM-7900F) equipped with an energy-dispersive X-ray spectroscopy device (EDS-Bruker Quantax XFlash® 6/30).

Funding

The author gratefully acknowledges the French National Centre for Scientific Research (CNRS), French German Research Institute of Saint-Louis (ISL, Saint-Louis, France) and University of Strasbourg (UNISTRA, Strasbourg, France) for funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Acknowledgments

The author thanks L. Josien and L. Vidal (IS2M, Mulhouse-F), and C. Nicollet (ISL, Saint-Louis-F), for the transmission and scanning electron microscopy analyses and the formulation of the energetic charges, respectively.

Conflicts of Interest

The author declares no conflict of interest.

References

  1. Agrawal, J.P. High Energy Materials–Propellants, Explosives, Pyrotechnics, 1st ed.; Wiley-VCH: Weinheim, Germany, 2010. [Google Scholar]
  2. Titov, V.M.; Anisichkin, V.F.; Mal’kov, I.Y. Synthesis of ultradispersed diamond in detonation waves. Combust. Explos. Shock Waves 1989, 25, 372–379. [Google Scholar] [CrossRef]
  3. Lu, Y.; Zhu, Z.; Liu, Z. Catalytic growth of carbon nanotubes through CHNO explosive detonation. Carbon 2005, 42, 361–370. [Google Scholar] [CrossRef]
  4. Cudzilo, S.; Maranda, A.; Nowaczewski, J.; Trebinski, R.; Trzcinski, W.A. Detonative synthesis of inorganic compounds. J. Mater. Sci. Lett. 2000, 9, 1997–2000. [Google Scholar] [CrossRef]
  5. Bukaemskii, A.A. Explosive synthesis of ultra-disperse aluminium oxide in an oxygen-containing medium. Combust. Explos. Shock Waves 2001, 37, 594–599. [Google Scholar] [CrossRef]
  6. Li, R.Y.; Li, X.J.; Yan, H.H.; Peng, J. Experimental Investigations of the controlled explosive synthesis of ultrafine Al2O3. Combust. Explos. Shock Waves 2013, 49, 105–108. [Google Scholar] [CrossRef]
  7. Qu, Y.; Li, X.; Wang, X.; Liu, D. Detonation synthesis of nanosized titanium oxide powders. Nanotechnology 2007, 18, 205602–205607. [Google Scholar] [CrossRef]
  8. Qu, Y.D.; Li, X.J.; Yan, H.H.; Ouyang, X. Selective synthesis of TiO2 nanopowders. Glass Phys. Chem. 2008, 34, 637–639. [Google Scholar] [CrossRef]
  9. Yan, H.; Zhao, T.; Li, X.; Zhao, B. Slurry explosive detonation synthesis and characterization of 10 nm TiO2. Ceram. Int. 2016, 42, 14862–14866. [Google Scholar] [CrossRef]
  10. Bukaemskii, A.A. Nanosize powder of zirconia. Explosive method of production and properties. Combust. Explos. Shock Waves 2001, 37, 481–485. [Google Scholar] [CrossRef]
  11. Da Silva, C.; Manuel, J.; Dos Santos, A.; Marisa, E. Nanometric-Sized Ceramic Materials, Process for their Synthesis and Uses Thereof. U.S. Patent 8557215, 15 October 2013. [Google Scholar]
  12. Dos Santos, A.; Marisa, E.; Da Silva, C.; Manuel, J.; Lagoa, C.; Cia, A.L. Process for Nanomaterial Synthesis from the Preparation and Detonation of an Emulsion, Products and Emulsions Thereof. U.S. Patent 9115001, 25 August 2015. [Google Scholar]
  13. Xie, X.; Li, X.; Zhao, Z.; Wu, H.; Qu, Y.; Huang, W. Growth and morphology of nanometer LiMn2O4 powder. Powder Technol. 2006, 169, 143–146. [Google Scholar] [CrossRef]
  14. Wang, X.H.; Li, X.J.; Yan, H.H.; Xue, L.; Qu, Y.D.; Sun, G.L. Nano-MnFe2O4 powder synthesis by detonation of emulsion explosive. Appl. Phys. A 2008, 90, 417–422. [Google Scholar] [CrossRef]
  15. Li, X.; Qu, Y.; Xie, X.; Wang, Z.; Li, R. Preparation of SrAl2O4: Eu2+, Dy3+ nanometer phosphors by detonation method. Mater. Lett. 2006, 60, 3673–3677. [Google Scholar] [CrossRef]
  16. Gibot, P.; Vidal, L.; Laffont, L.; Mory, J. Zirconia nanopowder synthesis via detonation of trinitrotoluene. Ceram. Intern. 2020, 46, 27057–27062. [Google Scholar] [CrossRef]
  17. Langenderfer, M.J.; Fahrenholtz, W.G.; Chertopalov, S.; Zhou, Y.; Mochalin, V.N.; Johnson, C.E. Detonation synthesis of silicon carbide nanoparticles. Ceram. Intern. 2020, 46, 6951–6954. [Google Scholar] [CrossRef]
  18. Medard, L. Les Explosives Occasionnels, 2nd ed.; Lavoisier Techniques & Documentation: Paris, France, 1999. [Google Scholar]
  19. Meyer, R.; Kohler, J.; Homburg, A. Explosives, 6th ed.; Wiley-VCH: Weinheim, Germany, 2007. [Google Scholar]
  20. Fischer, S.H.; Grubelich, M.C. Theoretical energy release of thermites, intermetallics, and combustible metals. In Proceedings of the 32nd AIAA/ASME/SAE/ASEE Joint Propulsion Conference, Lake Buena Vista, FL, USA, 1−3 July 1996. [Google Scholar]
  21. Gibot, P.; Goetz, V. Aluminium/Tin (IV) oxide thermite composite: Sensitivities and reaction propagation. J. Energ. Mater. 2020, 38, 295–308. [Google Scholar] [CrossRef]
  22. Pantoya, M.L.; Granier, J.J. Combustion behavior of highly energetic thermites: Nano versus Micron composites. Propellants Explos. Pyrotech. 2005, 30, 53–61. [Google Scholar] [CrossRef]
  23. Lowell, S.; Shields, J.E.; Thomas, M.A.; Thommes, M. Characterization of Porous Solids and Powders: Surface Area, Pore Size and Density, 1st ed.; Kluwer Academic Publishers: Dordrecht, The Netherlands, 2004. [Google Scholar]
  24. Akhavan, J. The Chemistry of Explosives, 2nd ed.; Royal Society of Chemistry: London, UK, 2004. [Google Scholar]
  25. Dolmatov, V.Y. Detonation synthesis nanodiamonds: Synthesis, structure, properties and applications. Russ. Chem. Rev. 2007, 76, 339–360. [Google Scholar] [CrossRef]
  26. Bastea, S. Nanocarbon condensation in detonation. Sci. Rep. 2017, 7, 42151. [Google Scholar] [CrossRef] [PubMed] [Green Version]
Figure 1. The energetic train (A) and the detonation chamber (B) used for the synthesis of oxide ceramics. The red cylinder in the detonation chamber represents the energetic train.
Figure 1. The energetic train (A) and the detonation chamber (B) used for the synthesis of oxide ceramics. The red cylinder in the detonation chamber represents the energetic train.
Ceramics 04 00019 g001
Figure 2. XRD patterns of the as-detonated oxide ceramics: (A) CeO2 (JCPDS card No. 01-081-0792), (B) HfO2 (JCPDS card No. 00-034-0104), (C) Nb2O5 (JCPDS cards No. 00-30-0873), and (D) In2O3 (JCPDS card No. 00-006-0416), respectively.
Figure 2. XRD patterns of the as-detonated oxide ceramics: (A) CeO2 (JCPDS card No. 01-081-0792), (B) HfO2 (JCPDS card No. 00-034-0104), (C) Nb2O5 (JCPDS cards No. 00-30-0873), and (D) In2O3 (JCPDS card No. 00-006-0416), respectively.
Ceramics 04 00019 g002
Figure 3. SEM (top) and TEM (down) images of the as-detonated (A) CeO2, (B) HfO2, (C) Nb2O5, and (D) In2O3 oxide ceramics, respectively.
Figure 3. SEM (top) and TEM (down) images of the as-detonated (A) CeO2, (B) HfO2, (C) Nb2O5, and (D) In2O3 oxide ceramics, respectively.
Ceramics 04 00019 g003
Figure 4. Nitrogen isotherms of the as-detonated ceramics: (A) CeO2, (B) HfO2, (C) Nb2O5 and (D) In2O3 materials, respectively. In the insert, the corresponding particle size distributions.
Figure 4. Nitrogen isotherms of the as-detonated ceramics: (A) CeO2, (B) HfO2, (C) Nb2O5 and (D) In2O3 materials, respectively. In the insert, the corresponding particle size distributions.
Ceramics 04 00019 g004
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Gibot, P. Synthesis of Oxide Ceramics in Detonating Atmosphere. Ceramics 2021, 4, 249-256. https://0-doi-org.brum.beds.ac.uk/10.3390/ceramics4020019

AMA Style

Gibot P. Synthesis of Oxide Ceramics in Detonating Atmosphere. Ceramics. 2021; 4(2):249-256. https://0-doi-org.brum.beds.ac.uk/10.3390/ceramics4020019

Chicago/Turabian Style

Gibot, Pierre. 2021. "Synthesis of Oxide Ceramics in Detonating Atmosphere" Ceramics 4, no. 2: 249-256. https://0-doi-org.brum.beds.ac.uk/10.3390/ceramics4020019

Article Metrics

Back to TopTop