Next Article in Journal
Field-Theoretic Simulations for Block Copolymer Melts Using the Partial Saddle-Point Approximation
Next Article in Special Issue
Lignosulphonates as an Alternative to Non-Renewable Binders in Wood-Based Materials
Previous Article in Journal
Tribological Performance and Thermal Stability of Nanorubber-Modified Polybenzoxazine Composites for Non-Asbestos Friction Materials
Previous Article in Special Issue
Binderless Thermal Insulation Panels Made of Spruce Bark Fibres
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Properties of Low-Cost WPCs Made from Alien Invasive Trees and rLDPE for Interior Use in Social Housing

by
Abubakar Sadiq Mohammed
and
Martina Meincken
*
Department of Forest and Wood Science, University of Stellenbosch, Private Bag X1, Matieland, Stellenbosch 7602, South Africa
*
Author to whom correspondence should be addressed.
Submission received: 8 July 2021 / Revised: 16 July 2021 / Accepted: 16 July 2021 / Published: 24 July 2021
(This article belongs to the Special Issue Recent Developments in Eco-Friendly Wood-Based Composites II)

Abstract

:
Low-cost wood–plastic composites (WPCs) were developed from invasive trees and recycled low-density polyethylene. The aim was to produce affordable building materials for low-cost social housing in South Africa. Both raw materials are regarded as waste materials, and the subsequent product development adds value to the resources, while simultaneously reducing the waste stream. The production costs were minimised by utilising the entire biomass of Acacia saligna salvaged from clearing operations without any prior processing, and low-grade recycled low-density polyethylene to make WPCs without any additives. Different biomass/plastic ratios, particle sizes, and press settings were evaluated to determine the optimum processing parameters to obtain WPCs with adequate properties. The water absorption, dimensional stability, modulus of rupture, modulus of elasticity, tensile strength, and tensile moduli were improved at longer press times and higher temperatures for all blending ratios. This has been attributed to the crystallisation of the lignocellulose and thermally induced cross-linking in the polyethylene. An increased biomass ratio and particle size were positively correlated with water absorption and thickness swelling and inversely related with MOR, tensile strength, and density due to an incomplete encapsulation of the biomass by the plastic matrix. This study demonstrates the feasibility of utilising low-grade recycled polyethylene and the whole-tree biomass of A. saligna, without the need for pre-processing and the addition of expensive modifiers, to produce WPCs with properties that satisfy the minimum requirements for interior cladding or ceiling material.

Graphical Abstract

1. Introduction

Alien invasive plants (AIP) in South Africa have enormous adverse consequences on biodiversity and ecosystem services and have led to direct environmental degradation [1,2]. With their high affinity for water and far-reaching roots and rapid spread, they often deplete water resources and degrade the soil, thereby water-stressing other plants and eventually alienating native flora and fauna in a local ecosystem. This has prompted the South African government to commit to a program aimed at clearing the most invasive plants. The cleared biomass is typically left behind to dry, where it poses a fire risk or, at best, is used as firewood. The issue of what to do with the biomass apart from the utilisation of fractions as firewood has emerged as a matter of concern.
Similarly, the surge in plastic pollution and its impact on the health and safety of ecosystems [3,4,5] is demanding attention. Plastic disposal in landfills results in leakages into the natural environment and consequently has dire adverse effects on wildlife, while incineration releases poisonous emissions. Plastic is therefore increasingly recycled, although the South African recycling industry is not quite as well developed as in Europe.
Making wood plastic composite (WPC) materials from these materials adds value to two different waste streams and can alleviate the financial burden of the government in managing these wastes and potentially form an employment- and income-generating enterprise by reprocessing them into secondary materials [5,6].
In South Africa, the government is trying to rectify the imbalance of property ownership caused by apartheid. Through the Reconstruction and Development Program (RDP), low-cost social housing units—called RDP houses—are being built across the country to address the enormous housing deficits [7,8]. However, the occupants of these budget houses are often exposed to the hazards of environmental stressors, such as heat and humidity, due to the low-quality of the building materials used [9]. The walls typically consist of a single-layer brick wall, without any additional insulation. Moisture condenses on the walls, resulting in mould, which increases their susceptibility to biodegradation and compromises the indoor air quality and health of occupants. The roofs are also often leaky, dripping water onto mostly wood or gypsum ceiling boards, which become soaking wet, develop discolouration, swell out of proportion, and deteriorate in a short time. These houses typically require maintenance shortly after construction, which the occupants cannot afford, resulting in undesirable living standards. Consequently, the use of interior ceiling and wall cladding materials that are high in hydrophobic properties to resist wetting-induced biodegradation while offering extended service lives is necessary. Interior cladding also offers the additional benefits of thermal and acoustic insulation against extreme weather conditions and community noise, which is typical in densely populated RDP settlements.
Utilising abundantly available recycled waste materials in the form of recycled low-density polyethylene (rLDPE) and AIPs as feedstock to develop low-cost WPC boards as wall cladding and ceiling material in RDP houses would add significantly to the living standard in these houses. The cost of the WPC materials is minimised by avoiding any unnecessary processing steps or additives and by using widely available raw materials that are otherwise regarded as waste materials that need to be removed. Recycled LDPE was chosen because of its abundant availability and low cost, as one of the main objectives was to keep the processing and manufacturing costs as low as possible. The recycled polymer was nominally linear low-density polyethylene (LLDPE), which has approximately the same density as LDPE, but with the linearity of HDPE and fairly short polymer chains. However, the obtained polymer was of the lowest quality. The plastic is sorted based on its polymer code and ranked into three quality grades—A, B, and C—in descending order. A-grade plastic is clean material generally sourced from shopping centres and recycled into pellets used for non-food packaging, such as refuse bags, furniture coverings, etc. C-grade is contaminated plastic that is often used in composite materials. Because of the impurities and the uncertainty of the exact composition, we refer to the recycled plastic material as rLDPE, rather than LLDPE.
After over a century since their first introduction, WPCs have evolved from wood-thermoset resin mixtures [10], through in-situ polymerization of plastic monomers within wood pores [10,11], to various blends of woody particles with thermoplastic polymers, as new thermoplastics with new properties and new technologies are continuously emerging [12]. The adhesion mechanism and bond strength between wood and plastic have been found to largely depend on the interlocking mechanism of a continuous plastic matrix through the wood cell lumen and intercellular pores, rather than the chemical bonds between polar wood cells and non-polar plastic [12,13,14]. Non-woody biomass, such as bark and leaves, are typically considered contaminants and avoided, because they generally lack the properties necessary for strength and bond formation [12,15,16]. Though leaves, bark, and twigs typically contain high amounts of lignin, which add stability, these are offset by the higher amounts of hemicelluloses, compared to woody biomass. Hemicelluloses are loosely bound non-crystalline fibres that oxidise easily and show a low thermal stability [12,13]. The inclusion of non-woody biomass into composites may thus lower their mechanical and thermal stability. In addition, leaves and bark are known to have a high extractive content [13,14,17]. Extractives are known to be rich in functional groups and affect the surface chemistry of wood [18]. Consequently, the bonds in WPC blends that depend on functional groups on the biomass surface may be enhanced by utilising biomass with a large extractive content. However, since polymers are largely unipolar, the majority of the bonds between wood and polymer rely on mechanical interlocking, rather than on chemical adhesion [12,19,20]. Contaminants may, however, add to the performance of WPCs. The higher lignin content in leaves and bark contributes to the moisture resistance, dimensional stability, and durability of composites [21,22] due to the hydrophobic nature of lignin and therefore provides some resistance against biological decay.
In recent reports, various kinds of non-wood lignocellulosic materials, including corncobs, nut shells [23], banana fibres [24], bamboo [25,26], rice husks [27], and many other unconventional biomass types, have found a use in WPC formulations. Owing to their chemical incompatibility, various protocols of pre-treatments have been applied in order to enhance interfacial bonding between biomass and plastic [13,14,28], which led to the introduction of coupling agents, such as maleic anhydride-grafted polypropylene (MAPP), Poly(ethylene-co-vinyl alcohol) (EVOH), and Polyethylene-graft maleic anhydride (PE-g-MA) to enhance bond strength [10,14,29]. However, coupling agents are costly and immensely increase the production costs of WPCs.
To manufacture WPC boards, temperatures between 140–200 °C [16,21,22,25,30] and press times between 5–30 min [17,23,24,31,32] are typically used. These press parameters significantly affect the properties of the WPCs. The upper and lower bound press temperature and time are usually given by the degradation temperature of the biomass type and the melting temperature of the thermoplastic [10,11,16,18]. Within these parameters are many possible combinations of processing settings, which affect the product properties.
Reports on the effect of biomass particle sizes and geometry on the properties of the resulting WPC boards are conflicting. Whereas some researchers report an improvement in some properties and a decrease in other properties with decreasing particle sizes [12,18,33,34,35], others conclude that particle size is less important to the final board properties than particle geometry [12,25,34,36,37]. Particle size reportedly affects the viscosity and melt flow rate during board formation [30,37,38] and consequently determines board–moisture relations.
Blending ratios between polymer matrix and wood reinforcements or fillers have been widely investigated [21,34,37,38,39,40,41] Depending on the intended properties and production method, ratios between 10% biomass, where the wood particles act as a filler in a continuous plastic matrix, and 90%, where the plastic acts as a binder, rather than a continuous matrix, have been reported. The biomass content at the higher extremes is usually the sole preserve of compression moulding methods, while the lower extremes may be injection moulded or extruded. A higher wood ratio generally results in an increased strength and stiffness, but it may also result in an increased moisture sorption and risks of microbial invasion [24,42].
In a previous study, the use of biomass obtained from A. saligna, A. mearnsii and E. camaldulensis—all invasive trees in South Africa—to produce WPCs was investigated [43]. The biomass was added in two forms: wood only and particles obtained by chipping and milling the entire tree with leaves, twigs, and bark. The results showed that regardless of the biomass type, WPCs made with A. saligna had superior mechanical properties, while composites with wood-only biomass were found to have better mechanical properties than composites with whole-tree biomass. In order to explain the superior properties of A. saligna, a chemical analysis was conducted on these species to identify the origin of the different properties of the resulting WPCs. Furthermore, it was essential to determine the optimum processing parameters to make WPC boards from entire trees of A. saligna and rLDPE. Consequently, different wood to plastic ratios and particle sizes were analysed, as well as different press temperatures and times. The physical and mechanical properties of the resulting WPC boards were analysed, and the effect of processing parameters on the performance of the final composites was determined.

2. Materials and Methods

2.1. Materials

Acacia saligna (Port Jackson) was obtained from clearing operations in the Western Cape of South Africa. Without any further processing, the trees were chipped, including wood, bark, leaves, seeds, and twigs, and air-dried (Figure 1a). The resulting biomass was passed through a 2 mm screen in a hammer mill and further air-dried to about 12% MC. Low-grade recycled low density polyethylene (rLDPE) consisting mostly of recycled shopping bags conglomerates, shown in Figure 1b, with a density of 0.915–0.950 g/cm3, was sourced from Atlantic Plastic Recycling (APR) CC, a plastic waste recycling plant in Cape Town, South Africa.

2.2. Composite Preparation

The biomass was chipped in an OC1 knife chipper (Figure 2a) from Heemaf, Netherlands and milled in a S1 hammermill from Drotsky, South Africa (Figure 2b) to a 2 mm particle size. The raw materials were mixed at three different biomass to plastic ratios—50:50, 60:40, and 70:30—and subsequently compounded in a custom built blender, shown in Figure 2c. The blending process resulted in a frictional breakdown of the WPC granules (Figure 3a), which were size separated into two fractions and characterised according to the procedure described in Section 2.3, from which the WPC boards were pressed.
The WPC granules were hot pressed at 150 and 180 °C for 10 and 30 min alternately in a hydraulic press from BURKLE, Germany in a 25 × 25 × 4 mm mould, shown in Figure 2d). The resulting boards shown in Figure 3b) were labelled with a three-digit sample code, where the first digit denotes the wood content (5, 6 and 7 = 50, 60 and 70 wt.%), the second letter identifies the particle size (S = 0.31 mm and L = 0.47), and the third letter (A, B, C, or D) identifies the time–temperature combination, where A: t = 10 min and T = 150 °C; B: t = 30 min and T = 150 °C; C: t = 10 min and T = 180 °C; and D: t = 30 min and T = 180 °C. Table 1 lists the processing parameters.

2.3. Size Analysis of Dry-Compounded Feedstock

Blending of the rLDPE and biomass in a rotary drum compounder resulted in a further frictional fractionation into particle sizes, which are a function of the blending time. The raw materials were compounded for 45 and 90 min, resulting in two different particle fractions designated as ‘L’ for larger particles from the 45 min compounding time and ‘S’ for the smaller graded particles obtained from the 90 min blending cycle. For a better description of the particle size distribution, samples of 150 g from the compounded feedstock were characterised through sieve analysis in an AS 200 shaker from Retsch, Germany the details of which are presented in Figure 4, indicating D50 as the particle diameter below which 50% of the particles were located.

2.4. Physical Properties

The specimens were conditioned at 20 °C and a 65% ± 5% relative humidity for 4 weeks, prior to testing. Two boards were produced for each treatment, and eight samples per treatment were tested to obtain a mean and a standard deviation. The moisture content (MC) was determined in accordance with ASTM D4442-07, using Equation (1):
M C   ( % ) = O r i g i n a l   m a s s ( g ) O v e n d r y   m a s s ( g ) O v e n d r y   m a s s ( g ) × 100  
The water absorption (WA) and thickness swell (TS) of 16 samples per treatment were carried out in accordance with ASTM D1037-12. The specimens were immersed in distilled water for 24 h, 7-, 14-, 21-, and 28-day immersion periods. At the end of each immersion period, the specimens were removed from the water and weighed to the nearest 0.01 g, and their thickness was measured with a digital calliper to the nearest 0.01 mm. The values for WA were calculated according to Equation (2):
W A t   ( % ) = W t W 0 W 0 × 100
where WAt is the water absorption (%) at time t. W0 and Wt are the respective weights of the specimens prior to immersion and after a given immersion time t.
TS was determined according to Equation (3):
T S t   ( % ) = D t D 0 D 0 × 100
where TSt is the thickness swelling (%) at time t. D0 and Dt are the respective thicknesses of the specimens prior to immersion and after a given immersion time t.
The board densities were determined according to Equation (4), as prescribed by ASTM standard D2395 (2014):
Density   ( ρ ) = O v e n d r y   m a s s a i r d r i e d   v o l u m e

2.5. Chemical Properties

The compositional analysis of the biomass from Acacia saligna, Acacia mearnsii, and Eucalyptus camaldulensis was conducted in accordance with the standards, NREL (LAP) TP-510-42620, TP-510-42622, TP-510-42621, TP-510-42618, and TP-510-42623 (2008) for ash content, hot water- and ethanol-soluble extractives (setup shown in Figure 5), lignin, sugar, and bulk density in order to determine how the composition affects the physical properties and performance of the WPCs.

2.6. Mechanical Properties

2.6.1. Static Bending

Four samples per treatment with a size of 195 × 50 × 4 mm were tested in a three-point bending test in accordance with ASTM D 1037-12 using a universal testing machine from Hottinger Baldwin Messtechnik (HBM), Germany (Figure 6a). The modulus of rupture (MOR) and modulus of elasticity (MOE) were determined according to Equations (5) and (6). All the calculated values are reported as the averages with the standard deviation.
M O R = 3 P m a x L 2 b d 2
M O R = L 3 4 b d 3 Δ P Δ y

2.6.2. Tensile Tests

Five dumbbell shaped samples with a size of 165 × 20 × 4 mm per treatment were tested in the tensile mode in accordance with ASTM D 638-14 using an Universal testing machine 4411 from Instron, Maine, USA equipped with a 5 kN load cell (Figure 6b), at a test speed of 50 mm/min. The tensile strength and tensile modulus were calculated based on Equations (7) and (8), and the average values are reported with the standard deviation.
T S = P m a x b d
E t = l g b d Δ P Δ y

2.7. Statistical Analysis

A factorial ANOVA with a replicates test in Statistica software 14.0.0.15 was used to determine significant differences within and between treatments at a significance level of α = 0.05. Pearson’s correlation analysis was conducted in R to quantify the contribution of all the independent variables on the physical properties of the boards.

3. Results

The findings from a previous study by Acheampong et al. [43], analysing WPCs made of biomass obtained from the whole tree or only the wood from A. saligna, A. mearnsii and E. camaldulensis, showed that the addition of bark, twigs, and leaves reduces the mechanical properties somewhat, but all boards still met the minimum requirements for interior use. A surprising finding, however, was that regardless of the biomass type, boards made with A. saligna showed significantly better mechanical properties than those made with the other two wood species. This was an unexpected result, especially the large difference between the two—otherwise very similar—Acacia species. To better understand the differences in performance, the chemical composition of the three different wood species was determined.

3.1. Chemical Composition

The chemical composition of the wood from A. saligna, A. mearnsii, and E. camaldulensis is presented in Table 2. A. saligna had the highest cellulose content of the three species, but with a low hemicelluloses content and average lignin content. The superior mechanical properties of WPCs made with A. saligna can be attributed to the high cellulose content, as the crystalline cellulose fibres are known to impart strength. The total extractive content of A. saligna was higher than that of the other two species and appeared to have no negative effect on the strength properties. On the contrary, the increased extractive content seemed to have aided the bonding between the biomass and the polymer matrix.
Based on the chemical composition and the results from Acheampong et al. [43], boards for further analysis were made from the entire tree of A. saligna, and the processing parameters were optimised to obtain the best physical and mechanical properties.

3.2. Water Absorption (WA) and Thickness Swelling (TS)

Observations at 24 h WA of all WPCs (Figure 7) indicate that regardless of the compounding ratio and particle size, the water absorption of all treatment ‘A’ samples pressed at T = 150 °C and t = 10 min was the highest, while the WA of treatment ‘D’ samples pressed at T = 180 °C and t = 30 min was the lowest. This is because at 180 °C, the biomass acquires a hydrophobic character due to thermal modification, which leads to the bonding of amorphous hydroxyl groups and a reduction of the available bonding sites for water [44,45]. The higher temperature also leads to a reduction in the melt–flow viscosity of rLDPE [14,46]. With a melt temperature of maximum 140 °C, the melt flow rates of the rLDPE at 180 °C would have been high. An increased flow rate and extended pressing time will increase the potential of the polymer to infiltrate the cell wall micro pores, impregnate the cell lumen and encrust entire particles, therefore decreasing the water absorption. At 150 °C, however, which is barely above the melting temperature of the rLDPE, the plastic remained more viscous and left more hydroxyl groups on the wood fibre surface exposed as potential binding sites for water [16,46,47]. While an increase in either the press time (treatment B) or temperature (treatment C) resulted in a reduced WA, there was no clear trend as to which of the two factors has more impact in reducing WA. However, increasing both factors resulted in the lowest WA.
Figure 7 shows the WA for small (S-series) and large particles (L-series) at increasing biomass ratios. The trend indicates that an increase in the biomass ratio from 50–70% resulted in a linear increase in WA from below 15% to over 20%. As the biomass is hydrophilic and the plastic is hydrophobic, an increase in the biomass to plastic ratio means more available potential binding sites for water, which will increase the WA.
Similar to the observed trends in WA, the TS (Figure 8) was independent of the particle size, and the longest pressing time and highest temperature resulted in the lowest TS across all blending ratios. While the increase in the press temperature or time alone resulted in an increased dimensional stability, none of the two factors showed any superiority over the other; however, the effect of the combined increase in press temperature and time resulted in the lowest TS (below 2%).
The short-term (2 h) and long-term (672 h) WA and TS for the various press settings (A–D) are presented in Table 2 for all blending ratios and particles sizes. As can be seen, the moisture absorption for press temperatures of T = 150 °C and t = 10 min (A) was the largest, particularly for WPC samples with a 70% biomass, which exceeded 30% MC after water immersion for 672 h. At press settings of T = 180 °C and t = 30 min (D), the lowest WA was recorded. WPCs made with larger particles generally absorbed more water than those made with smaller particles.
Board densities (Table 3) are a direct function of the blending ratio affected by the press temperature and time combination. Samples with a 50% biomass were consistently denser for all press settings (A–D) than WPCs made with 60% or 70% biomass, which had the lowest density. The presence of non-woody biomass in the form of leaves, twigs, and bark significantly reduced the density of the entire biomass below that of the rLDPE. The leaves with their characteristically thin cell walls, numerous intercellular spaces, and loosely packed spongy cells may not have contributed much to the weight but contributed enormously to the bulk volume of the biomass. Consequently, an increase in the biomass ratio resulted in an increase in the filler volume, without a proportionate increase in the mass. The combined effect of a high temperature at 180 °C and longer press time at 30 min under a 250 kg/cm2 pressure created a suitable condition for a reduced shear viscosity and improved the melt flow rate of the rLDPE, which generally has a melting temperature of 140 °C. The resulting boards were thus more compressed due to the better plastic melt-flow kinetics, and the smaller sized biomass particles allowed for a better compaction and improved the densification [15,35]. At a 70% biomass content, however, the plastic played the role of a binder, rather than a matrix. Since the biomass has a lower density than the plastic, a plastic weight ratio of 30% resulted in a much lower volume ratio, compared to the biomass. This disproportionate volume ratio implied that longer pressing times and higher press temperature were required for the plastic to melt and wet the biomass fibre surfaces, before successfully binding the particles together.
From the Pearson’s correlation matrices shown in Figure 9, the blending ratio (B. ratio) has the highest correlation (0.78) for WA among all the independent input variables and is therefore the most important determinant of water absorption. Since TS is a direct function of WA, as seen from Figure 9, the dimensional stability of the boards is also largely impacted by the blending ratio. As the press time and temperature are increased, WA and TS are decreased. Figure 7 and Figure 8 do not show clearly which of these two variables has a more significant impact on WA and TS. However, in Figure 9, it can be seen that temperature has a larger effect on the reduction of WA and TS than time. While press time is negatively correlated with TS, the correlation is not statistically significant. The effect of particle size on both WA and TS is also significant and positively correlated. Press temperature and time bear no significant correlation with density on their own, but the combined effect is significant. However, the blending ratio correlates positively with density. The board density shows a linear relation with WA and an inverse relation with TS.

3.3. Mechanical Properties

3.3.1. Static Bending Strength

The results of the strength modulus of 3-point bending tests for all treatments are presented in Figure 10. For each blending ratio across particle sizes, the highest MOR is obtained for treatment ‘D’ samples pressed at T =180 °C and t = 30 min, while the lowest strength values were obtained for treatment ‘A’ samples pressed at T = 150 °C and t = 10 min. The effect of increasing the time (B) or temperature (C) alone resulted in an increase in strength, but there was no clear trend in terms of which of the two variables has a greater impact on strength. However, the increased press time and temperature together resulted in the highest board strength. This can be explained by the formation of a continuous polymer matrix around the biomass fibres and occupation of intercellular voids. The densified composite will have fewer micro pores and fewer stress concentration points and therefore an increased strength.
Boards with a 50% biomass had the highest bending strength properties, with a maximum MOR of about 23 MPa. As the biomass content increased, the MOR was reduced and showed the lowest value of 13 MPa at 70%. This can be explained by the inhomogeneity of the biomass, which contained fibres from leaves, twigs, and bark, which have a lower content of crystalline cellulose and higher portions of short fibres containing amorphous hemicelluloses and lignin. On the whole, boards made with a smaller particle size biomass (S) show slightly higher strengths than larger particles (L), although the difference is not statistically significant. This can be explained by the better flow of the polymer around smaller particles, which leads to a continuous matrix.

3.3.2. Flexural MOE

Figure 11 illustrates the bending stiffness of the WPC boards. Similar to the MOR, samples ‘D’ pressed at T = 180 °C and t = 30 min showed a superior bending stiffness for all blending ratios and particle sizes, while treatment samples ‘A’ pressed at T = 150 °C and t = 10 min recorded the lowest stiffness. As observed before, an increase in either the temperature or time of pressing resulted in an increase in stiffness, but without a clear trend regarding which of the two variables had a greater impact. However, unlike the MOR, composites with a higher biomass content at 70% show the highest bending stiffness, exceeding 900 MPa, and boards with a 50% biomass recorded the lowest stiffness. This indicates that the main contributor to stiffness is the biomass, which acts as a reinforcement in the composite. The impact of particle size on bending stiffness did not follow a clear trend, even though comparative observations of treatment ‘A’ and ‘D’ samples across particle sizes indicate that smaller particle sizes generally had better bending moduli.

3.3.3. Tensile Strength

The tensile strength of the WPC boards is illustrated in Figure 12 and shows a positive linear relationship with increasing press temperature and/or time. This trend can be explained by the more efficient matrix formation of the rLDPE around the biomass particles. The sustained elevated temperatures above the melt temperature of the rLDPE rendered it less viscous and improved its flow and diffusion into the cell wall micro pores to form continuous matrices, thus imparting a higher tensile strength. An inverse relationship between the tensile strength and biomass ratio was observed across particle sizes. At a higher biomass loading, the composite samples had a higher stiffness due to the reinforcing impact of the biomass. Consequently, an increase in the tensile load broke the samples with a higher biomass ratio at smaller strain levels. With a reduction in the biomass content, the WPCs gained elasticity, which resulted in a higher tensile strength. This phenomenon was observed across particle sizes. However, no clear trend regarding the independent effect of particle size on tensile strength could be statistically established.

3.3.4. Tensile MOE

The observed tensile moduli were not very different from the tensile strength. From Figure 13, it is observed that treatment ‘D’ samples pressed at T = 180 °C and t = 30 min had a significantly higher tensile modulus than treatment ‘A’ samples pressed at T = 150 °C and t = 10 min for all blending ratios. This may be attributed to the re-crystallisation of cellulose, in addition to the realignment of lignin at a higher temperature and extended pressing time. However, an increase in the biomass ratio resulted in a rise in tensile stiffness, with the lowest stiffness recorded at approximately 230 MPa for a biomass ratio of 50% wt. and the highest stiffness of nearly 400 MPa at a 70% biomass ratio. The tensile modulus of the WPC is therefore largely determined by the blending ratio and press time and temperature. The effect of particle size generally showed no clear trend. However, the comparative analysis of treatment ‘A’ and ‘D’ samples across particle sizes suggests that the WPCs made with larger particles had higher tensile moduli.

4. Discussion

Given that cellulose plays an important role in bond formation [17,37,48], the higher content of cellulose in A. saligna suggests its higher potential for wood-polymer bond formation. However, this also implies a more hygroscopic character of the composite. This correlation between cellulose content and a high moisture uptake is confirmed by several researchers [12,15,18,31,47,49,50]. In order to maximise the full benefits of a high cellulose content, while simultaneously limiting the disadvantages, the press conditions that promote an efficient biomass encapsulation by the hydrophobic plastic are required. This is achieved at temperatures above the melting point of the plastic and a sufficient press time to allow for an effective flow, wetting, and diffusion into biomass. This can be observed in Figure 7, Figure 8, Figure 9, Figure 10, Figure 11, Figure 12 and Figure 13 and Table 3, which show that the elevated temperature and longer press time create better conditions to lower the viscosity of the plastic, therefore allowing it to reach into inter-particle crevices and cell lumina. The resulting formation of a continuous plastic matrix enhances the biomass particle encapsulation, which inhibits the bonding of water molecules to the free hydroxyl groups of holocellulose [15,47,50]. Subsequently, a reduction in water absorption and improvement in dimensional stability are achieved. This is further facilitated by the plasticisation of lignin and the conformational reorganisation of holocellulose due to the dehydration reactions of residual water resulting from the exposure of the biomass to high press temperature conditions [44,45,51]. These findings have been confirmed by several other researchers [14,52], who noted that the choice of press temperature and time affect the melt temperature and melt flow rates of the plastic and the thermal degradation temperature of the biomass [16,29]. The combination of the press temperature and blending ratio ultimately determines the extent of the particle encapsulation within the plastic matrix.
Extractives play a crucial role in wood–plastic bond formation. Polyphenolics and terpenes, including suberin and resin compounds, have hydrophobic functional groups with a considerable influence on the surface chemistry of wood [12,53,54,55]. Since a higher surface energy is required for a good bonding between biomass and polyethylene, a lower extractive content reduces the potential of wood–plastic adhesion via chemical bonds, while promoting mechanical interlocking. Some components of wood extractives oxidise and form volatiles upon exposure to air and light during drying and subsequent heat exposure during processing. This potentially lowers the surface energy of the biomass as extractives, particularly tannins, which are known to be present in considerable quantities in A. saligna, contribute largely to bond formation and water repellence. The reduced surface energy translates into a reduction in the adhesion potential [14,15,52]. At optimised press temperatures, however, extractives do not entirely escape, but migrate to the surfaces of the biomass, where they increase the adhesion between the plastic and biomass. As extractives migrate to the surface, they leave behind micro-voids, which, given sufficient press time will be filled by the plastic matrix through diffusion, which is a slow process [17,50,51,56]. The eventual wood–plastic bonds are both chemical at the interface and mechanical at the cell wall level. The high amount of extractives contained in the leaves and bark of the biomass also act as a plasticiser and can considerably reduce the viscosity of the plastic and enhance the particle dispersion in WPC processing [51,55,57,58]. These properties collectively enhance the moisture resistance of the composite products. Consequently, forming WPCs with biomass high in extractives requires the optimisation of the press settings to maximise both the benefits of the chemical adhesion via a surface energy boost, as well as mechanical interlocking.
At higher temperatures and longer press times, the hemicellulose concentration of the biomass, particularly of the leaves and twigs, may have either partially or wholly degraded. Boonstra et al. [59], Ates et al. [60] and Phuong et al. [61] have reported that the degradation of hemicelluloses starts below 200 °C. Inari et al. [62] found through X-ray photoelectron spectroscopy that after heat treatment at around 200 °C, the hydroxyl concentration of the wood surface decreased due to the thermal degradation of the hemicelluloses. Since the hydrophilic properties of wood depend on an amount of available hydroxyl groups, a reduction in the concentration of these functional groups results in an increased hydrophobic character of the wood [63]. These findings are corroborated by Hakkou et al. [45], Gérardin et al. [64], and Chaouch et al. [65], who reported that the oxygen to carbon ratio of wood at the surface decreases with increasing temperatures above 120 °C. This reduction in the O/C concentration ratio is accompanied by a reduction in the concentration of polar wood components due to dehydration reactions, the depolymerisation of amorphous holocellulose, and the selective degradation of hydroxyl groups. These reactions induce moisture resistance; however, they also lower the surface free energy of biomass and negatively affect wood polymer adhesion [17,59,66], while aiding apolar bonds [64].
Composites pressed at a higher temperature and time exhibited better mechanical properties. Thermal modification is known to induce crosslinks within wood and plastic, which explains the improvement of the mechanical properties. The increase in the stiffness of the WPCs with increasing temperature is in good agreement with the findings of other researchers, such as Lyutyy et al. [67] and Santos [68]. Kubojima et al. [69] noted that the MOE and MOR of wood increases for the first 30 min of heat treatment at 160 °C, after which it begins to decline. This has been attributed to lignin relocation and the re-crystallisation of cellulose [61]. However, the positive correlation between the increased press temperature and mechanical strength observed in this study was not confirmed by Hakkou et al. [45], Korkut et al. [70], or Bal and Bektaş [71], who reported that heating wood above 120 °C hindered the mechanical properties.
It was also observed that the dimensional stability and mechanical properties of the WPCs were better in samples made with smaller particles, irrespective of the compounding ratio. This can be explained by the more continuous matrix formation around the smaller particles. This observation is confirmed by various other studies [16,33,35,47,52], where the effect of the biomass particle size on the WPC properties was analysed. Smaller particles also result in better compressibility during hot pressing, which eliminates inter-particle voids and reduces the porosity of the composite. The enhanced compressibility also impacts directly on the board density, as better compaction results in a higher board density [30,35,72,73].
The blending ratio had the most significant effect on the board properties. The presence of lightweight non-woody particles, such as leaves and porous bark, lowers the overall density of the biomass, resulting in composites with lower densities as the biomass content increases. The lower biomass density results in a disproportionately higher biomass volume per weight, which reduces the potential of the plastic to wet, infiltrate, and encapsulate the proportionately larger volume of the biomass. Since the resistance of WPCs to moisture sorption, and an effective stress transfer is reliant on the interaction between the stiffer hydrophilic biomass and the ductile hydrophobic polymer, the pathways for moisture movement into the composites and stress concentration points are higher in an incomplete biomass particle enclosure. Consequently, the blending ratio between wood and plastic needs to be adjusted according to the intended application. At a 50% biomass ratio, there is enough plastic to provide moisture resistance, but the boards are less rigid and have a higher density, which is not desirable for insulation boards. Boards with a 60% biomass fraction display a good balance between moisture resistance, strength, and medium density, with thermo-acoustic insulation benefits for interior use [74].

5. Conclusions

WPC boards were made in a cost-effective way, without prior processing of the biomass, such as debarking, separating non-woody and woody parts, or the use of additives, such as compatibilisers. The recycled plastic was the lowest grade—and therefore cheapest—rLDPE. The resulting boards had physical and mechanical properties comparable to commercial products used for insulation purposes and met all the requirements for non-structural interior applications in buildings. The long-term WA and TS results suggest that the panels may be used in high-humidity interior environments, such as kitchens, without much risk of biodegradation and deformation, while the density and mechanical properties make them suitable for interior wall cladding and ceiling boards. All the investigated processing factors—blending ratio, particle size, press time, and temperature—were found to significantly affect the board properties, albeit to varying degrees. The blending ratio is the most important determinant of physical and mechanical properties. A higher press temperature and longer press times lower the viscosity of the plastic and improve the melt-flow rates, while also re-crystallising the cellulose fibres. This gives rise to stronger bonds between the plastic and biomass and a better encapsulation of the biomass particles. However, the maximum temperature is limited to prevent thermal degradation of the biomass. WPC boards made with smaller particle fractions showed better physical and mechanical properties due to a better encapsulation of the biomass particles by the plastic matrix, which leads to improved hydrophobic properties. However, the improvement in the mechanical properties was not as notable.
Ultimately, boards made with a 60% biomass ratio and pressed at 180 °C for 30 min showed the best balance between mechanical and physical properties for interior applications. The obtained density is sufficient but not too high to allow for a good thermo-acoustic insulation.

Author Contributions

Conceptualization: A.S.M. and M.M.; methodology: A.S.M.; formal analysis: A.S.M.; resources: M.M.; writing—original draft preparation: A.S.M.; writing—review and editing: M.M. Both authors have read and agreed to the published version of the manuscript.

Funding

The project on which this work is based was funded by the German Federal Ministry of Education and research, under the grant No. 01DG17007A and in the DAAD project 57359374. The authors are responsible for the content of this publication.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

All data is available upon request.

Acknowledgments

The authors wish to thank TKC Amandla for the harvesting and transport of the invasive trees and Atlantic Recycling for the provision of rLDPE.

Conflicts of Interest

The authors declare no conflict of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript, or in the decision to publish the results.

References

  1. Wilson, J.R.U.; Ivey, P.; Manyama, P.; Nänni, I. A new national unit for invasive species detection, assessment and eradication planning. S. Afr. J. Sci. 2013, 109, 1–13. [Google Scholar] [CrossRef] [Green Version]
  2. Van Wilgen, B.W.; Reyers, B.; Le Maitre, D.C.; Richardson, D.M.; Schonegevel, L. A biome-scale assessment of the impact of invasive alien plants on ecosystem services in South Africa. J. Environ. Manag. 2008, 89, 336–349. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  3. Wilcox, C.; Van Sebille, E.; Hardesty, B.D.; Estes, J.A. Threat of plastic pollution to seabirds is global, pervasive, and increasing. Proc. Natl. Acad. Sci. USA 2015, 112, 11899–11904. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  4. Jambeck, J.; Geyer, R.; Wilcox, C.; Siegler, T.R.; Perryman, M.; Andrady, A.; Narayan, R.; Law, K.L. Plastic waste inputs from land into the ocean. Mar. Pollut. 2015, 347, 768–771. [Google Scholar] [CrossRef] [PubMed]
  5. WEF. The New Plastics Economy: Rethinking the Future of Plastics; WEF: Geneva, Swizerland, 2016; Available online: https://www.ellenmacarthurfoundation.org/assets/downloads/publications/NPEC-Hybrid_English_22-11-17_Digital.pdf (accessed on 2 May 2020).
  6. Geyer, R.; Jambeck, J.R.; Law, K.L. Production, use, and fate of all plastics ever made. Sci Adv. 2017, 3, 25–29. [Google Scholar] [CrossRef] [Green Version]
  7. Department of Human Settlement. National Housing Policy and Subsidy Programmes; Department of Human Settlement: Pretoria, South Africa, 2010. [Google Scholar]
  8. Krickova, A. Reconstruction and Development Programme as a tool of socio-economic transformation. Modern Africa Polit. Hist. Soc. 2015, 3, 57–93. [Google Scholar]
  9. Manomano, T.; Tanga, P.T. Housing needs: The quality and quantity of housing provided by the government for the poor in the Eastern Cape province in South Africa. Soc. Work 2018, 54, 19–36. [Google Scholar] [CrossRef]
  10. Clemons, C. Interfacing wood-plastic composites industries in the U.S. For. Prod. J. 2002, 52, 10–18. [Google Scholar]
  11. Li, Y. Wood-polymer composites. In Advances in Composite Materials—Analysis of Natural and Man-Made Materials; Tesinova, P., Ed.; IntechOpen: Shanghai, China, 2011; pp. 229–284. Available online: http://www.intechopen.com/books/advances-in-composite-materials-analysis-of-natural-and-man-madematerials/%0Awood-polymer-composites (accessed on 9 September 2020).
  12. Stokke, D.D.; Gardner, D.J. Fundamental aspects of wood as a component of thermoplastic composites. J. Vinyl Addit. Technol. 2003, 9, 96–104. [Google Scholar] [CrossRef]
  13. Cho, J.D.; Kim, S.G.; Hong, J.W. Surface modification of polypropylene sheets by UV-radiation grafting polymerization. J. Appl. Polym. Sci. 2006, 99, 1446–1461. [Google Scholar] [CrossRef]
  14. Van Der Leeden, M.C.; Frens, G. Surface properties of plastic materials in relation to their adhering performance. Adv. Eng. Mater. 2002, 4, 280–289. [Google Scholar] [CrossRef]
  15. Schneider, M.H. Wood Polymer Composites. Wood Fiber Sci. 1994, 26, 142–151. [Google Scholar]
  16. Clemons, C.M.; Caufield, D.F. Wood flour. In Functional Fillers for Plastics; Xanthos, M., Ed.; Wiley-VCH Verlag GmbH & Co KgaA: Weinheim, Germany, 2005; pp. 249–270. [Google Scholar]
  17. Vassilev, S.V.; Baxter, D.; Andersen, L.K.; Vassileva, C.G.; Morgan, T.J. An overview of the organic and inorganic phase composition of biomass. Fuel 2012, 94, 1–33. [Google Scholar] [CrossRef]
  18. Farmer, R.H. Chemistry in the Utilization of Wood, 1st ed.; Pergamon Press Ltd.: London, UK, 1967; pp. 1–183. [Google Scholar] [CrossRef]
  19. Migneault, S.; Koubaa, A.; Perré, P.; Riedl, B. Effects of wood fiber surface chemistry on strength of wood-plastic composites. Appl. Surf. Sci. 2015, 343, 11–18. [Google Scholar] [CrossRef]
  20. Frihart, C.R.; Hunt, C.G. Adhesives with wood materials: Bond formation and performance. In Wood Handbook—Wood as an Engineering Material; General Technical Report FPL-GTR-190; Centennial Ross, R.J., Ed.; Forest Products Laboratory: Madison, WI, USA, 2010; pp. 228–251. [Google Scholar]
  21. Irle, M.; Barbu, M.C. Wood-based panel technology. In Wood-Based Panels—An Introduction for Specialists; Thoemen, H., Irle, M., Sernek, M., Eds.; Brunel University Press: London, UK, 2010; pp. 1–94. [Google Scholar]
  22. Reddy, K.O.; Uma Maheswari, C.; Muzenda, E.; Shukla, M.; Rajulu, A.V. Extraction and Characterization of Cellulose from Pretreated Ficus (Peepal Tree) Leaf Fibers. J. Nat. Fibers 2016, 13, 54–64. [Google Scholar] [CrossRef]
  23. Ogah, A.O.; Elom, N.I.; Ngele, S.O.; Nwofe, P.A.; Agbo, P.E.; Englund, K.R. Water Absorption, Thickness Swelling and Rheological Properties of Agro Fibers/HDPE Composites. IOSR J. Polym Text. Eng. 2015, 2, 66–73. [Google Scholar] [CrossRef]
  24. Liu, H.; Wu, Q.; Zhang, Q. Preparation and properties of banana fiber-reinforced composites based on high density polyethylene (HDPE)/Nylon-6 blends. Bioresour. Technol. 2009, 100, 6088–6097. [Google Scholar] [CrossRef] [PubMed]
  25. Hung, K.C.; Yeh, H.; Yang, T.C.; Wu, T.L.; Xu, J.W.; Wu, J.H. Characterization of wood-plastic composites made with different lignocellulosic materials that vary in their morphology, chemical composition and thermal stability. Polymers 2017, 9, 726. [Google Scholar] [CrossRef] [Green Version]
  26. Dehghan, M.; Faezipour, M.; Azizi, M.; Hosseinabadi, H.Z.; Bari, E.; Nicholas, D.D. Assessment of physical, mechanical, and biological properties of bamboo plastic composite made with polylactic acid. Maderas Cienc. Tecnol. 2019, 21, 599–610. [Google Scholar] [CrossRef] [Green Version]
  27. Ayrilmis, N.; Kaymakci, A.; Akbulut, T.; Elmas, G.M. Mechanical performance of composites based on wastes of polyethylene aluminum and lignocellulosics. Compos. Part B Eng. 2013, 47, 150–154. [Google Scholar] [CrossRef]
  28. Effah, B.; Van Reenen, A.; Meincken, M. Mechanical properties of wood-plastic composites made from various wood species with different compatibilisers. Eur. J. Wood Wood Prod. 2018, 76, 57–68. [Google Scholar] [CrossRef]
  29. Frihart, C.R. Wood adhesion and adhesives. In Handbook of Wood Chemistry and Wood Composites; Rowell, R.M., Ed.; CRC Press: Boca Raton, FL, USA, 2005; pp. 219–282. [Google Scholar]
  30. Hosseinihashemi, S.K.; Modirzare, M.; Safdari, V.; Kord, B. Decay resistance, hardness, water absorption, and thickness swelling of a bagasse fiber/plastic composite. BioResources 2011, 6, 3289–3299. [Google Scholar] [CrossRef]
  31. Zabihzadeh, S.M. Water uptake and flexural properties of natural filler/HDPE composites. BioResources 2010, 5, 316–323. [Google Scholar] [CrossRef]
  32. Jayamani, E.; Hamdan, S.; Ezhumalai, P.; Soon, K.H. Acoustic and thermal properties of polymer composites reinforced with lignocellulosic fibers. Appl. Mech. Mater. 2014, 624, 25–29. [Google Scholar] [CrossRef]
  33. Bouafif, H.; Koubaa, A.; Perré, P.; Cloutier, A. Effects of fiber characteristics on the physical and mechanical properties of wood plastic composites. Compos. Part A Appl. Sci. Manuf. 2009, 40, 1975–1981. [Google Scholar] [CrossRef]
  34. AlMaadeed, M.A.; Nógellová, Z.; Janigová, I.; Krupa, I. Improved mechanical properties of recycled linear low-density polyethylene composites filled with date palm wood powder. Mater. Des. 2014, 58, 209–216. [Google Scholar] [CrossRef]
  35. Adefisan, O.O.; McDonald, A.G. Evaluation of the strength, sorption and thermal properties of bamboo plastic composites. Maderas Cienc. Tecnol. 2019, 21, 3–14. [Google Scholar] [CrossRef] [Green Version]
  36. Krause, K.C.; Sauerbier, P.; Koddenberg, T.; Krause, A. Utilization of recycled material sources for wood-polypropylene composites: Effect on internal composite structure, particle characteristics and physico-mechanical properties. Fibers 2018, 6, 86. [Google Scholar] [CrossRef] [Green Version]
  37. Migneault, S.; Koubaa, A.; Erchiqui, F.; Chaala, A.; Englund, K.; Wolcott, M.P. Effects of processing method and fiber size on the structure and properties of wood-plastic composites. Compos. Part A Appl. Sci. Manuf. 2009, 40, 80–85. [Google Scholar] [CrossRef]
  38. Ozdemir, F.; Ayrilmis, N.; Kaymakci, A.; Kwon, J.H. Improving dimensional stability of injection molded wood plastic composites using cold and hot water extraction methods. Maderas Cienc. Tecnol. 2014, 16, 365–372. [Google Scholar] [CrossRef] [Green Version]
  39. Pelaez-Samaniego, M.R.; Yadama, V.; Lowell, E.; Amidon, T.E.; Chaffee, T.L. Hot water extracted wood fiber for production of wood plastic composites (WPCs). Holzforschung 2013, 67, 193–200. [Google Scholar] [CrossRef]
  40. Adhikary, K.B.; Pang, S.; Staiger, M.P. Dimensional stability and mechanical behaviour of wood-plastic composites based on recycled and virgin high-density polyethylene (HDPE). Compos. Part B Eng. 2008, 39, 807–815. [Google Scholar] [CrossRef]
  41. Stark, N.M.; Cai, Z.; Carll, C. Wood-Based Composite Materials Panel Products, Glued-Laminated Timber, Structural Materials. In Wood Handbook—Wood as an Engineering Material; General Technical Report, FPL-GTR-190; Centennial Ross, R.J., Ed.; Wood Products Laboratory: Madison, WI, USA, 2010; pp. 252–279. [Google Scholar]
  42. Luo, Z.; Li, P.; Cai, D.; Chen, Q.; Qin, P.; Tan, T.; Cao, H. Comparison of performances of corn fiber plastic composites made from different parts of corn stalk. Ind. Crops Prod. 2017, 95, 521–527. [Google Scholar] [CrossRef]
  43. Acheampong, J.B.; de Angelis, M.; Krause, A.; Meincken, M. The effect of raw material selection on physical and mechanical properties of wood plastic composites made from recycled LDPE and wood from invasive trees in South Africa. Wood Mater. Sci. Eng. 2021, 16, 118–123. [Google Scholar] [CrossRef]
  44. Rowell, R.M. Moisture Properties. In Handbook of Wood Chemistry and Wood Composites; Rowell, R.M., Ed.; CRC Press: Boca Raton, FL, USA, 2005; pp. 84–106. [Google Scholar]
  45. Hakkou, M.; Pétrissans, M.; Zoulalian, A.; Gérardin, P. Investigation of wood wettability changes during heat treatment on the basis of chemical analysis. Polym. Degrad. Stab. 2005, 89, 1–5. [Google Scholar] [CrossRef]
  46. Wang, M.-L.; Chang, R.-Y.; Hsu, C.-H. Material properties of plastics. In Laser Welding of Plastics, 1st ed.; Klein, R., Ed.; Wiley-VCH Verlag GmbH & Co. KGaA: Weinheim, Germany, 2011; pp. 3–69. [Google Scholar]
  47. Kallakas, H.; Poltimäe, T.; Süld, T.M.; Kers, J.; Krumme, A. The influence of accelerated weathering on the mechanical and physical properties of wood-plastic composites. In Proceedings of the Estonian Academy of Sciences, 2015; Estonian Academy Publishers: Tallinn, Estonia, 2015; Volume 64, pp. 94–104. [Google Scholar] [CrossRef]
  48. Gulitah, V.; Liew, K.C. Three different recycle codes of plastic/Acacia fibre composites: Physical and morphological properties. Int. J. Biobased Plast. 2019, 1, 1–7. [Google Scholar] [CrossRef] [Green Version]
  49. Wechsler, A.; Hiziroglu, S. Some of the properties of wood-plastic composites. Build. Environ. 2007, 42, 2637–2644. [Google Scholar] [CrossRef] [Green Version]
  50. Tabarsa, T.; Khanjanzadeh, H.; Pirayesh, H. Manufacturing of wood-plastic composite from completely recycled materials. Key Eng. Mater. 2011, 471–472, 62–66. [Google Scholar] [CrossRef]
  51. Wiedenhoeft, A. Structure and function of wood. In Wood Handbook: Wood as an Engineering Material; General Technical Report, FPL-GTR-19; Centennial Ross, R.J., Ed.; Forest Products Laboratory: Madison, WI, USA, 2010; pp. 62–79. Available online: www.fpl.fs.fed.us (accessed on 30 May 2021).
  52. Gallagher, L.W.; McDonald, A.G. The effect of micron sized wood fibers in wood plastic composites. Maderas Cienc Tecnol. 2013, 15, 357–374. [Google Scholar] [CrossRef] [Green Version]
  53. Clemons, C. Raw materials for wood-polymer composites. In Composites Science and Engineering, Wood-Polymer Composites; Niska, K.O., Sain, M., Eds.; Woodhead Publishing: Sawston, UK, 2008; pp. 1–22. [Google Scholar] [CrossRef]
  54. Leskinen, T.; Salas, C.; Kelley, S.S.; Argyropoulos, D.S. Wood Extractives Promote Cellulase Activity on Cellulosic Substrates. Biomacromolecules 2015, 16, 3226–3234. [Google Scholar] [CrossRef]
  55. Jansson, M.B.; Nilvebrant, N.-O. Wood extractives. In Pulp and Paper Chemistry and Technology: Wood Chemistry and Wood Biotechnology; Ek, M., Gellerstedt, G., Henriksson, G., Eds.; Walter de Gruyter GmbH & Co.: Berlin, Germany, 2009; Volume 1, pp. 147–171. [Google Scholar]
  56. Klyosov, A.A. Wood-Plastic Composites; John Wiley & Sons, Inc.: Hoboken, NJ, USA, 2007; pp. 1–696. [Google Scholar]
  57. Rowell, R.M.; Pettersen, R.; Han, J.S.; Rowell, J.S.; Tshabalala, M.A. Cell Wall Chemistry. In Handbook of Wood Chemistry and Wood Composites; Rowell, R.M., Ed.; CRC Press: Boca Raton, FL, USA, 2005; pp. 43–82. [Google Scholar]
  58. Clemons, C.M.; Stark, N.M. Feasibility of using saltcedar as a filler in injection-molded polyethylene composites. Wood Fiber Sci. 2009, 41, 2–12. [Google Scholar]
  59. Boonstra, M.J.; Van Acker, J.; Kegel, E.; Stevens, M. Optimisation of a two-stage heat treatment process: Durability aspects. Wood Sci. Technol. 2007, 41, 31–57. [Google Scholar] [CrossRef]
  60. Ates, S.; Hakan, A.M.; Ozdemir, H. Heat-Treated Calabrian Pine Wood. BioResources 2009, 4, 1032–1043. [Google Scholar]
  61. Phuong, L.X.; Shida, S.; Saito, Y. Effects of heat treatment on brittleness of Styrax tonkinensis wood. J. Wood Sci. 2007, 53, 181–186. [Google Scholar] [CrossRef]
  62. Inari, G.N.; Petrissans, M.; Lambert, J.; Ehrhardt, J.J.; Rardin, P.G. XPS characterization of wood chemical composition after heat-treatment. Surf. Interface Anal. 2006, 38, 1380–1385. [Google Scholar] [CrossRef]
  63. Pétrissans, M.; Gérardin, P.; El Bakali, I.; Serraj, M. Wettability of heat-treated wood. Holzforschung 2003, 57, 301–307. [Google Scholar] [CrossRef]
  64. Gérardin, P.; Petrič, M.; Petrissans, M.; Lambert, J.; Ehrhrardt, J.J. Evolution of wood surface free energy after heat treatment. Polym. Degrad. Stab. 2007, 92, 653–657. [Google Scholar] [CrossRef]
  65. Chaouch, M.; Pétrissans, M.; Pétrissans, A.; Gérardin, P. Use of wood elemental composition to predict heat treatment intensity and decay resistance of different softwood and hardwood species. Polym. Degrad. Stab. 2010, 95, 2255–2259. [Google Scholar] [CrossRef]
  66. Mitsui, K.; Inagaki, T.; Tsuchikawa, S. Monitoring of hydroxyl groups in wood during heat treatment using NIR spectroscopy. Biomacromolecules 2008, 9, 286–288. [Google Scholar] [CrossRef]
  67. Lyutyy, P.; Bekhta, P.; Sedliacik, J.; Ortynska, G. Properties of flat-pressed wood-polymer composites made using secondary polyethylene. Acta Fac Xylologiae 2014, 56, 39–50. [Google Scholar]
  68. Santos, J.A. Mechanical behaviour of Eucalyptus wood modified by heat. Wood Sci. Technol. 2000, 34, 39–43. [Google Scholar] [CrossRef]
  69. Kubojima, Y.; Okano, T.; Ohta, M. Bending strength and toughness of heat-treated wood. J. Wood Sci. 2000, 46, 8–15. [Google Scholar] [CrossRef]
  70. Korkut, S.; Akgül, M.; Dündar, T. The effects of heat treatment on some technological properties of Scots pine (Pinus sylvestris L.) wood. Bioresour. Technol. 2008, 99, 1861–1868. [Google Scholar] [CrossRef] [PubMed]
  71. Bal, B.C.; Bektaş, I. The Effects of Heat Treatment on Some Mechanical Properties of Juvenile Wood and Mature Wood of Eucalyptus grandis. Dry Technol. 2013, 31, 479–485. [Google Scholar] [CrossRef]
  72. Rahman, K.S.; Islam, M.N.; Rahman, M.M.; Hannan, M.O.; Dungani, R.; Khalil, H.P.S.A. Flat-pressed wood plastic composites from sawdust and recycled polyethylene terephthalate (PET): Physical and mechanical properties. Springerplus 2013, 2, 1–7. [Google Scholar] [CrossRef] [Green Version]
  73. Chen, H.C.; Chen, T.Y.; Hsu, C.H. Effects of wood particle size and mixing ratios of HDPE on the properties of the composites. Holz Roh Werkst 2006, 64, 172–177. [Google Scholar] [CrossRef] [Green Version]
  74. Wang, W.; Morrell, J.J. Water sorption characteristics of two wood-plastic composites. For. Prod. J. 2004, 54, 209–212. [Google Scholar]
Figure 1. (a) Milled whole-tree biomass of A. saligna and (b) rLDPE.
Figure 1. (a) Milled whole-tree biomass of A. saligna and (b) rLDPE.
Polymers 13 02436 g001
Figure 2. (a) Knife chipper, (b) hammermill, (c) custom-built blender, and (d) hydraulic press.
Figure 2. (a) Knife chipper, (b) hammermill, (c) custom-built blender, and (d) hydraulic press.
Polymers 13 02436 g002
Figure 3. (a) Dry-compounded feedstock and (b) sample board, after hot-pressing at 180 °C for 30 min.
Figure 3. (a) Dry-compounded feedstock and (b) sample board, after hot-pressing at 180 °C for 30 min.
Polymers 13 02436 g003
Figure 4. Particle size distribution, showing the variation in D50 as a function of the compounding time.
Figure 4. Particle size distribution, showing the variation in D50 as a function of the compounding time.
Polymers 13 02436 g004
Figure 5. Soxhlet extraction setup for biomass compositional analysis.
Figure 5. Soxhlet extraction setup for biomass compositional analysis.
Polymers 13 02436 g005
Figure 6. Instron setup for (a) the 3-point bending test, and (b) tensile test.
Figure 6. Instron setup for (a) the 3-point bending test, and (b) tensile test.
Polymers 13 02436 g006
Figure 7. A 24 h WA of WPCs pressed at different temperatures and times (A–D) with 50, 60, and 70% biomass at two particle sizes (S and L).
Figure 7. A 24 h WA of WPCs pressed at different temperatures and times (A–D) with 50, 60, and 70% biomass at two particle sizes (S and L).
Polymers 13 02436 g007
Figure 8. A 24 h TS of WPCs pressed at different temperatures and times (A–D) with 50, 60, and 70% biomass at two particle sizes (S and L).
Figure 8. A 24 h TS of WPCs pressed at different temperatures and times (A–D) with 50, 60, and 70% biomass at two particle sizes (S and L).
Polymers 13 02436 g008
Figure 9. Pearson’s R correlations of the impact of independent press parameters on the physical properties (WA, TS and density) of WPCs. The correlation matrices marked (x) are not significant or inapplicable.
Figure 9. Pearson’s R correlations of the impact of independent press parameters on the physical properties (WA, TS and density) of WPCs. The correlation matrices marked (x) are not significant or inapplicable.
Polymers 13 02436 g009
Figure 10. Flexural strength (MOR) of the WPCs pressed at different temperatures and times (A–D) with 50, 60, and 70% biomass at two particle sizes (S and L). Symbols with the same letters are not significantly different.
Figure 10. Flexural strength (MOR) of the WPCs pressed at different temperatures and times (A–D) with 50, 60, and 70% biomass at two particle sizes (S and L). Symbols with the same letters are not significantly different.
Polymers 13 02436 g010
Figure 11. Flexural MOE of the WPCs pressed at different temperatures and times (A–D) with 50, 60, and 70% biomass at two particle sizes (S and L).
Figure 11. Flexural MOE of the WPCs pressed at different temperatures and times (A–D) with 50, 60, and 70% biomass at two particle sizes (S and L).
Polymers 13 02436 g011
Figure 12. Tensile strength of the WPCs pressed at different temperatures and times (A–D) with 50, 60, and 70% biomass at two particle sizes (S and L). Symbols with the same letters are not significantly different.
Figure 12. Tensile strength of the WPCs pressed at different temperatures and times (A–D) with 50, 60, and 70% biomass at two particle sizes (S and L). Symbols with the same letters are not significantly different.
Polymers 13 02436 g012
Figure 13. Tensile MOE of the WPCs pressed at different temperatures and times (A-D) with 50, 60, and 70% biomass at two particle sizes (S and L).
Figure 13. Tensile MOE of the WPCs pressed at different temperatures and times (A-D) with 50, 60, and 70% biomass at two particle sizes (S and L).
Polymers 13 02436 g013
Table 1. Blending ratios and time–temperature-mix treatments of WPCs at S (0.31 mm) and L (0.47) particle sizes.
Table 1. Blending ratios and time–temperature-mix treatments of WPCs at S (0.31 mm) and L (0.47) particle sizes.
Blending
Ratio
(wt. %)
Particle size S Pressure
(kg/cm2)
Particle Size L
Press
Temperature
(°C)
Press Time
(min)
Sample CodePress
Temperature
(°C)
Press Time
(min)
Sample Code
50:50150105SA2500150105LA
305SB305LB
180105SC180105LC
305SD305LD
60:40150106SA150106LA
306SB306LB
180106SC180106LC
306SD306LD
70:30150107SA150107LA
307SB307LB
180107SC180107LC
307SD307LD
Table 2. Compositional analysis of the wood of A. saligna, A. mearnsii, and E. camaldulensis.
Table 2. Compositional analysis of the wood of A. saligna, A. mearnsii, and E. camaldulensis.
Parameters (%)Biomass Type
A. salignaA. mearnsiiE. camaldulensis
Lignin19.69 (0.48)18.92 (0.57)21.14 (1.96)
Hemicelluloses15.18 (0.69)16.24 (0.10)17.36 (1.23)
Cellulose41.97 (2.54)35.55 (0.49)28.74 (2.34)
Water Extractives7.62 (0.41)6.02 (1.22)4.85 (0.78)
Ethanol Extractives0.18 (0.19)0.15 (0.09)0.18 (0.04)
Total Extractives7.80 (0.19)6.17 (0.92)5.03 (0.64)
Ash1.07 (0.47)1.30 (0.76)0.93 (0.08)
Values in parenthesis are the standard deviations.
Table 3. Board density ( ρ ) and WA and TS of the WPCs made with small (S) and large (L) particle sizes at different blending ratios after 2 h, 24 h, and 672 h.
Table 3. Board density ( ρ ) and WA and TS of the WPCs made with small (S) and large (L) particle sizes at different blending ratios after 2 h, 24 h, and 672 h.
TreatmentSample
Code a
ρ
(g/cm3)
WA (h)TS (h)Sample
Code a
ρ
(g/cm3)
WA (h)TS (h)
224672224672 224672224672
A5SA1.613.27
(0.23)
14.43
(1.34)
30.76
(2.44)
4.39
(0.39)
7.03
(0.60)
9.60
(0.55)
5LA1.493.68
(0.17)
11.71
(0.56)
29.64
(0.83)
2.56
(0.27)
4.30
(0.37)
8.40
(0.68)
6SA0.935.27
(0.12)
12.54
(0.38)
33.96
(0.62)
1.42
(0.06)
5.10
(0.20)
9.30
(0.30)
6LA0.945.70
(0.27)
19.01
(1.44)
37.46
(1.86)
3.79
(0.25)
6.23
(0.52)
8.94
(0.58)
7SA0.9610.69
(0.19)
22.81
(0.28)
37.05
(0.45)
5.70
(0.15)
8.74
(0.40)
11.46
(0.32)
7LA0.7611.40
(0.18)
22.63
(0.34)
37.40
(1.44)
4.76
(0.05)
8.27
(0.07)
12.06
(0.12)
B5SB1.522.84
(0.15)
10.10
(0.33)
30.53
(0.83)
3.99
(0.14)
4.54
(0.42)
6.91
(0.60)
5LB1.542.50
(0.08)
10.37
(0.54)
28.18
(1.09)
0.71
(0.05)
2.61
(0.15)
6.26
(0.35)
6SB1.012.65
(0.06)
9.23
(0.20)
30.30
(0.59)
0.65
(0.03)
3.57
(0.16)
6.49
(0.31)
6LB0.972.95
(0.08)
10.63
(0.28)
35.58
(0.85)
0.43
(0.02)
3.70
(0.20)
7.19
(0.32)
7SB0.938.72
(0.44)
22.65
(1.68)
34.09
(2.39)
3.89
(0.22)
7.17
(0.53)
9.61
(0.71)
7LB0.888.30
(0.22)
21.07
(0.95)
34.87
(1.76)
2.53
(0.05)
6.87
(0.23)
10.79
(0.31)
C5SC1.462.79
(0.10)
6.83
(0.31)
27.39
(2.28)
3.15
(0.34)
4.57
(0.47)
6.86
(0.63)
5LC1.392.97
(0.12)
8.62
(0.36)
27.36
(0.74)
0.65
(0.04)
1.95
(0.10)
5.90
(0.27)
6SC1.122.73
(0.05)
9.77
(0.11)
31.02
(0.25)
1.30
(0.06)
4.49
(0.17)
6.95
(0.26)
6LC0.973.82
(0.09)
11.86
(0.23)
32.67
(0.86)
2.30
(0.16)
4.91
(0.35)
7.55
(0.47)
7SC0.975.24
(0.11)
14.79
(0.34)
29.76
(0.51)
3.51
(0.18)
6.97
(0.25)
9.65
(0.34)
7LC0.898.91
(0.29)
21.72
(0.88)
35.87
(1.71)
4.12
(0.17)
7.95
(0.22)
11.46
(0.33)
D5SD1.411.32
(0.04)
5.20
(0.17)
19.85
(0.82)
0.58
(0.03)
1.87
(0.09)
6.39
(0.29)
5LD1.472.43
(0.07)
8.53
(0.23)
24.45
(0.85)
0.50
(0.04)
1.70
(0.12)
5.64
(0.37)
6SD0.942.32
(0.07)
8.09
(0.28)
27.28
(0.81)
1.03
(0.04)
2.39
(0.09)
6.25
(0.16)
6LD1.062.26
(0.04)
8.50
(0.17)
27.88
(0.62)
1.14
(0.05)
3.43
(0.15)
5.84
(0.21)
7SD0.994.89
(0.12)
14.24
(0.30)
27.96
(0.67)
2.43
(0.06)
4.51
(0.14)
9.04
(0.25)
7LD0.896.62
(0.23)
19.48
(0.68)
30.18
(1.07)
2.39
(0.07)
6.21
(0.21)
10.23
(0.26)
a refer to Table 1 for the WPC treatment composition and corresponding codes. (Values in parenthesis are the standard deviations).
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Mohammed, A.S.; Meincken, M. Properties of Low-Cost WPCs Made from Alien Invasive Trees and rLDPE for Interior Use in Social Housing. Polymers 2021, 13, 2436. https://0-doi-org.brum.beds.ac.uk/10.3390/polym13152436

AMA Style

Mohammed AS, Meincken M. Properties of Low-Cost WPCs Made from Alien Invasive Trees and rLDPE for Interior Use in Social Housing. Polymers. 2021; 13(15):2436. https://0-doi-org.brum.beds.ac.uk/10.3390/polym13152436

Chicago/Turabian Style

Mohammed, Abubakar Sadiq, and Martina Meincken. 2021. "Properties of Low-Cost WPCs Made from Alien Invasive Trees and rLDPE for Interior Use in Social Housing" Polymers 13, no. 15: 2436. https://0-doi-org.brum.beds.ac.uk/10.3390/polym13152436

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.