Next Article in Journal
A Study on the Healing Performance of Solid Capsules for Crack Self-Healing of Cementitious Composites
Previous Article in Journal
Performance Analysis of DAST Material-Assisted Photonic-Crystal-Based Electrical Tunable Optical Filter
Previous Article in Special Issue
Growth and Characterization of Second and Third Order Acentric Studies of l-Phenylalanine l-Phenylalaninium Malonate Single Crystal
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Crystal Growth of RuS2 Using a Chemical Vapor Transport Technique and Its Properties

1
Laboratory of Semiconductors, Nanostructures and Advanced Technologies, Borj Cedria Science and Technology Park, BP 95, Hammam-Lif 2050, Tunisia
2
Departement de Physique, Faculté des Sciences de Bizerte, Université de Carthage, Tunis 7021, Tunisia
3
Groupe d’Etude de la Matière Condensée, CNRS-Université de Versailles St-Quentin 1, Place A, Briand, CEDEX, F-92195 Meudon, France
4
Department of Physics and Astronomy, King Saud University, Riyadh 11451, Saudi Arabia
*
Author to whom correspondence should be addressed.
Submission received: 13 June 2022 / Revised: 6 July 2022 / Accepted: 11 July 2022 / Published: 17 July 2022

Abstract

:
In this work, we study the effect of increasing temperature on the structure parameters (lattice, sulfur–sulfur distance, and ruthenium–sulfur distance) and the energy gap of RuS2. However, it was very challenging to obtain a sample of RuS2 due to many factors, some of which are discussed in the introduction. To prepare the crystal growth of RuS2, we have used the chemical vapor transport technique. The crystals obtained show a pyrite structure, of which we studied its crystallographic structure, including the structure of crystals in surface (100). The sample was then characterized by X-ray diffraction and by microprobe analysis. We determine the relationship between the energy gap and the sulfur–sulfur distance. We analyzed the S-S bond compared with the S2 molecule.

1. Introduction

The aim of this work is the study of the effect of the sulfur–sulfur distance on the electronic and optical properties of the R u S 2 pyrite. Over the past few years much attention has been given to the study of sulfur-containing compounds. This tendency is due to the increasing environmental issues, as well as academic interests [1]. Ruthenium Sulfide, Crystals 12 00994 i001 R u S 2 is one of the interesting sulfur compounds from both fundamental and technological points of view. It is one of the semiconducting transition-metal dichalcogenide (TMDC) materials, with a reported band gap of 1.8 eV [2] and has a pyrite structure [3]. Ruthenium Sulfide, R u S 2 has several possible uses, including its use as a catalyst [4] and as a photoelectrode [5,6,7,8]. However, it is difficult to obtain the crystalline R u S 2 due to several facts, for instance we can obtain R u S 2 only at temperatures greater than 1000 °C. Therefore, obtaining its crystalline structure at low temperatures is practically impossible. Moreover, the physical vapor transport method is difficult to use because the vapor pressure of R u S 2 is very low, at temperatures between 800 and 1050 ° C .
Our work is structured as follows. First, we provide a detailed description of the experimental procedure used to obtain R u S 2 by the chemical vapor transport technique. Next, we provide a brief description of the techniques and tools used to analyze the obtained sample, such as X-ray diffraction and microprobe analysis. In addition, we provide a detailed analysis of our findings; that is, the influence of increasing temperature on the stoichiometry shift of sulfur, S and how the different values of the energy gap helped us to understand and analyze the effect of other parameters, such us temperature, sulfur–sulfur distance, and ruthenium–sulfur distance on the energy gap. Moreover, and as one of our results demonstrates, we show the correlation between the sulfur–sulfur bond and energy gap.
The study of the surface is an important key toward understanding the effect of distribution of sulfur nanoparticles on the value of band gap. Finally, to further understand the interaction between the R u S 2 nanoparticles and surface bonding, we clarified the electronic processes that relate to the bonding in the surface of R u S 2 nanoparticles.

2. Experimental Section

In this work we carry out the chemical vapor transport (CVT) growth in a closed quartz ampule. The phase vapor transport is carried out using silica ampules containing R u S 2 powder and a very low percentage of sulfur. The ampule is 200 mm in length and 25 mm in diameter. The ampule is sealed under chlorine atmosphere (100 mm of Hg). We started crystallization of R u S 2 ; we used l C l 3 and S 2 C l 2 as transport agents. After, we introduced a small quantity of the oxygen form R u O 2 . In the end, the quantity of chlorine and R u O 2 determined 2 atmospheres of R u O C l 2 in total at 900 ° C . The R u O C l 2 was then annealed in a dynamical vacuum of 2 atmospheric pressures at a temperature of 900 ° C . The crystal growth took place in a graphite-covered quartz ampule.
The mixture R u S 2 + R u O 2 + C l 2 was used as the chemical agent to transport the material from the warm to the cool zone. The temperature of the source materials was between 900 °C and 1025 °C. The crystallization took place in the ampule where the temperature was reduced by 50   ° C after each crystallization. The growth region was situated in a hot zone, 925–1050 °C. The duration of transport was between 7 and 15 days. Mono-crystalline R u S 2 was formed in the cool zone of the ampule. By this method, we obtained a polycrystalline structure that consists of mono-crystal grains where the dimensions can decrease from 4 mm × 4 mm × 4 mm to   0.5   mm   × 0.2   mm × 0.2   mm . The color of the obtained crystal varies based on the temperature from dark gray to shiny light gray; our result is listed in Table 1.
We have noticed that the better quality of R u S 2 was obtained at the lowest temperature, which makes this technique of chemical vapor transport very interesting. The importance of this technique is the ability to lower the crystallization temperature of the most refractory materials.
Given the fact that the thermal stability of R u S 2 (Pdissociation = 5 mbar at T = 1100 °C) which is a high temperature. It is impossible to transport halides between 800 and 850 °C and that is since the vapor pressure of ruthenium containing species is low. So far, the CVT of R u S 2   has not been a successful growth method; for example, see [9]. However, for us we succeed in forming R u O x C l y when it is transported at a low temperature, and that is due the fact that we used oxygen from R u O 2 . Figure 1, shows the growth of monocrystal of R u S 2 by CVT.

3. Analysis

Several different single crystals of RuS2 grown by the above technique have been analyzed by microprobe and X-ray diffraction.

3.1. Analysis by Microprobe

We used microprobe casting (camera MS 46–CNRS de Bellevue), which provides a specific chemical analysis using an accelerated and focused electron beam on the sample (Φ < 1 μm at the surface of the sample). Under the effect of electron bombardment, the single crystal produces an X emission of lines characteristic of the elements present. The main reason for using microprobe casting is to observe the influence of both the chemical vapor transport method and the temperature increase in the stoichiometry shift of the sulfur (S) rich atmosphere. As expected, a significant influence on the obtained concentration of RuS2 was observed. In Table 2, we can see the heavy influence of temperature on the stoichiometry shift of sulfur, S. When the temperature increases, we do not obtain exactly RuS2, instead the quantity of sulfide slightly decreases, and therefore obtaining a sample of R u S 2 is challenging, as mentioned in the introduction.
In these preliminary results we have not observed the micro-weight of oxygen or anything chloric. It has been observed that as the temperature increases, sulfur concentration decreases, and the material becomes more nonstoichiometric: see Figure 2.
As can be seen, where the temperature increases, the stoichiometry shift of sulfur decreases.

3.2. Analysis by X-ray

Powder X-ray diffraction measurements were made on crushed crystals using a Philips diffractometer with CuK α radiation. Cell parameters were calculated, with the aid of a computer, using a least-squares refinement program. Selected crystals were also examined by microprobe casting. Powder X-ray diffraction patterns showed the cubic, with lattice parameters close to the literature value of 5.609 Å 5.635 Å [10], where RuS2 crystallizes as laurite in a pyrite type structure, in which disulfide ions are octahedrally coordinated to the Ru metal ion; having the space group symmetry Th6 (Pa3), the lattice parameters are the same as in ASTM file. The calculated experimental values for constant lattice a, parameter of structure ν , sulfur–sulfur distance d s - s and Ruthenium–sulfur distance d R u - s are listed in Table 3.
In terms of bond distances, we can see that the R u - S bond decreases from 2.373   Å   back to 2.367   Å . The S 2 pair is a weakening of the S - S bond, as the calculated bond length increases when the temperature increases from 900   ° C   to   1050   ° C . To recover the well-known bond character within the S 2 molecules. The S - S bond increases from 1.990   A ˙   to 2.118   A ˙ . The effect of the temperature to bonding in the R u S 2 . is shown in Figure 3 and Figure 4, which parameters of structure   ν define the atomic position of sulfur. Both the S - S and R u - S bonds increase with temperature. Thus, they conclude the influence of temperature to parameter structure ν , it is presented in Figure 4  ν increases when temperature increases. The precise bond for the structure (Ru-S and S-S distances) comes from the balance between the temperature and the method to prepare R u S 2 . Hence, we deduce that the structure of R u S 2 . depends heavily on the temperature.
Next, by using the results of our experimental work we provide more details about the relationship between the structure of RuS2 and the temperature, along with the effect of the temperature and the S - S bond on the gap energy.
We have determined that there are different values of the energy gap of   R u S 2 . These values are listed in Table 4 below. In Figure 5, we plotted ( α h ν ) 1 2 versus h ν photon energy. From this graph we conclude that pyrite R u S 2 is a semiconductor, has an indirect band gap, and different values of band gap.
The results show a clear and strong dependency of the energy gap on temperature (Figure 6a) and show an extraordinary decrease in the energy gap when the crystallization of the samples is carried out at high temperatures. It is also clear that when the excess of sulfur increases, the energy gap decreases (Figure 6b). However, we have determined the relationship between the growth parameters (temperature, lattice, and distance) and the energy gap. Table 5 shows that the S-S bond is in good agreement with crystallographic data and the elongation of the S-S bond compared with the S2 molecule. As the resulting energy gap decreases (from 1.68 to 1.25 eV), the sulfur–sulfur distance increases (from 1.990 to 2.118   A ˙ ). This clearly shows that the energy gap is strongly dependent on the S-S distance. However, all founded values of the energy gap have the same type of S-S bond in RuS2. Moreover, the interesting property of RuS2 is that, regardless of the change of the value of energy gap, it keeps pairs of sulfur S2 and not an individual S atom. In our study, the sample CS9 has smallest dimension, it was prepared at the lowest temperature of 900   ° C and it has the highest band gap 1.68   eV , which shows that the morphology of crystal R u S 2 strongly depends on the band gap and temperature, especially the distribution of sulfur, similar to the work carried out by Aqueel et al. in [11] where they showed the temperature effect on the morphology of C u C o 2 S 4 .
The pyrite structure of RuS2 is schematically shown in Figure 7a,b. From the two figures, we can see that the pyrite RuS2 presents as a face-centered cube of Ru. Figure 7c presents S 2 molecules, it is clear there are molecules similar to R u S 2 , which we have at the cube center, and in the middle of the cube edges (in R u S 2   molecules) S 2 molecules are located. However, RuS2 appears as S2 pairs coordinating a metal center. Each Ru atom is in an octahedral arrangement surrounded by six S2 molecules. Moreover, only one S of each pair is bonded to the Ru atom and the bonds from the metal atom are arranged in a distorted octahedron. Each S atom has three Ru neighbors, and a S2 pair has six metal neighbors in a pseudo-octahedral coordination. Figure 7d shows that R u S 2 has only the S-S bond type in this structure. Even that can show significant variation of energy gap values of RuS2, and it is therefore important to understand the S-S bond in the R u S 2 and how it affects the energy gap. This is why it is important to study the surface (100) of pyrite R u S 2 . The Figure 8 results show the structure of surface (100) and surface (110). It proved that small nanoparticles of sulfur are responsible for most properties. It shows the active sites that can react with surface and affect electron transmission. Ru atom has a d   electronic configuration [12] with low spin t 2 g where S atom has S   3 p state with up spin P P σ * . This motivated us to confirmed that band gap depends only the position of Sulfur (parameter of structure ν ) and S-S distance.

4. Conclusions

We have successfully prepared RuS2 by the chemical vapor transport method. Obtaining RuS2 at a low temperature is practically impossible [13]. We have determined the energy gap, and sulfur–sulfur distance for different samples. In conclusion, we can obtain RuS2 at a low temperature (900   ° C and 950   ° C ) with an important stoichiometry shift of sulfur, for samples CS9 and CS8.
Our work shows a strong dependence between the sulfur–sulfur distance and the energy gap on the temperature, which leads us to the conclusion that when the growth parameter increases, the energy gap decreases. Furthermore, our results have demonstrated that in comparison with the GaAS semiconductors in [14,15] pyrite R u S 2 has different gaps. Moreover, pyrite R u S 2 is the best candidate for multispectral solar cells.

Author Contributions

Conceptualization, R.S., O.G., H.E.; Investigation, R.S., E.A.A.; Validation, R.S., Writing (original draft), R.S., E.A.A., H.E.; Project administration, O.G., H.E.; Supervision, O.G., H.E.; Resources, O.G., H.E.; Software, E.A.A. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Acknowledgments

We would like to thank Laboratoire de Physique du Solide au CNRS de Bellevue (LPSB) for letting us use their lab for our experimental work.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Topsoe, H.; Clausen, B.S.; Massoth, F.E. Hydrotreating Catalysis-Science and Technology. Springer 1996, 14, 1465. [Google Scholar] [CrossRef]
  2. Hulliger, F. Crystal Structure and Electrical Properties of Some Cobalt-Group Chalcogenides. Nature 1964, 204, 644–646. [Google Scholar] [CrossRef]
  3. Knop, O.; Reid, K.I.G.; Sutarno; Nakagawa, Y. Chalkogenides of the transition elements. VI. X-ray, neutron, and magnetic investigation of the spinels Co3O4, NiCo2O4, Co3S4, and NiCo2S4. Can. J. Chem. 1968, 46, 22. [Google Scholar] [CrossRef] [Green Version]
  4. Harris, S.; Chianelli, R. Catalysis by transition metal sulfides: The relation between calculated electronic trends and HDS activity. J. Catal. 1984, 86, 400–412. [Google Scholar] [CrossRef]
  5. Ezzouia, H.; Heindl, R.; Parsons, R.; Tributsch, H. Visible light photo-oxidation of water with single-crystal RuS2 electrodes. J. Electroanal. Chem. Interfacial Electrochem. 1983, 145, 279–292. [Google Scholar] [CrossRef]
  6. Heindl, R.; Parsons, R.; Redon, A.; Tributsch, H.; Vigneron, J. Photoelectrochemical behaviour of ruthenium disulphide electrodes in contact with aqueous electrolytes. Surf. Sci. 1982, 115, 91–103. [Google Scholar] [CrossRef]
  7. Ezzaouia, H.; Heindl, R.; Loriers, J. Synthesis of ruthenium and osmium dichalcogenide single crystals. J. Mater. Sci. Lett. 1984, 3, 625–626. [Google Scholar] [CrossRef]
  8. Ezzaouia, H.; Foise, J.W.; Gorochov, O. Crystal growth in tellurium fluxes and characterization of RuS2 single crystals. Mater. Res. Bull. 1985, 20, 1353–1358. [Google Scholar] [CrossRef]
  9. Fiechter, S.; Kuhne, H.-M. Crystal growth of RuX2 (X = 5, Se, Te) by chemical vapour transport and high temperature solution growth. J. Cryst. Growth 1987, 83, 517–522. [Google Scholar] [CrossRef]
  10. Hulliger, F. Electrical Properties of Pyrite-Type and Related Compounds with Zero Spin Moment. Nature 1963, 200, 1064–1065. [Google Scholar] [CrossRef]
  11. Ahmed, A.T.A.; Chavan, H.S.; Jo, Y.; Cho, S.; Kim, J.; Pawar, S.M.; Gunjakar, J.L.; Inamdar, A.I.; Kim, H.; Im, H. One-step facile route to copper cobalt sulfide electrodes for supercapacitors with high-rate long-cycle life performance. J. Alloy. Compd. 2017, 724, 744–751. [Google Scholar] [CrossRef]
  12. Sai, R.; Gorochov, O.; Ezzaouia, H. The study of the electronic structure of RuS2. Results Phys. 2021, 26, 104393. [Google Scholar] [CrossRef]
  13. Castillo-Villalón, P.; Ramírez, J.; Maugé, F. Structure, stability and activity of RuS2 supported on alumina. J. Catal. 2008, 260, 65–74. [Google Scholar] [CrossRef]
  14. Spirkoska, D.; Efros, A.L.; Lambrecht, W.R.L.; Cheiwchanchamnangij, T.; Fontcuberta i Morral, A.; Abstreiter, G. Valence band structure of polytypic zinc-blende/wurtzite GaAs nanowires probed by polarization-dependent photoluminescence. Phys. Rev. B 2012, 85, 045309. [Google Scholar] [CrossRef] [Green Version]
  15. Cheiwchanchamnangij, T.; Lambrecht, W. Band structure parameters of wurtzite and zinc-blende GaAs under strain in the GW approximation. Phys. Rev. B 2011, 84, 035203. [Google Scholar] [CrossRef]
Figure 1. Growth of monocrystal of RuS2 by CVT.
Figure 1. Growth of monocrystal of RuS2 by CVT.
Crystals 12 00994 g001
Figure 2. The effect of temperature on sulfur concentration.
Figure 2. The effect of temperature on sulfur concentration.
Crystals 12 00994 g002
Figure 3. Sulfur–sulfur distance versus temperature.
Figure 3. Sulfur–sulfur distance versus temperature.
Crystals 12 00994 g003
Figure 4. Parameter of structure ν versus temperature.
Figure 4. Parameter of structure ν versus temperature.
Crystals 12 00994 g004
Figure 5. ( α h ν ) 1 2 versus h v .
Figure 5. ( α h ν ) 1 2 versus h v .
Crystals 12 00994 g005
Figure 6. (a) Band gap versus temperature, (b) band gap versus stoichiometric shift of Sulfur.
Figure 6. (a) Band gap versus temperature, (b) band gap versus stoichiometric shift of Sulfur.
Crystals 12 00994 g006
Figure 7. (a) crystallographic structure of Pyrite R u S 2 , (b) crystallographic structure of pyrite R u S 2 , (c) crystallographic structure of pyrite S 2 ,   and (d) primitive cell of RuS2.
Figure 7. (a) crystallographic structure of Pyrite R u S 2 , (b) crystallographic structure of pyrite R u S 2 , (c) crystallographic structure of pyrite S 2 ,   and (d) primitive cell of RuS2.
Crystals 12 00994 g007
Figure 8. Distribution of sulfur in the surface (100) and the surface (110) of the pyrite R u S 2 .
Figure 8. Distribution of sulfur in the surface (100) and the surface (110) of the pyrite R u S 2 .
Crystals 12 00994 g008
Table 1. The change of the color of grain crystal. This change is associated with a percentage of concentration of sulfur and the temperature. Additionally, the color of crystals related to the dimension of the grain. However, we succeeded in obtaining RuS2 by the chemical vapor transport technique.
Table 1. The change of the color of grain crystal. This change is associated with a percentage of concentration of sulfur and the temperature. Additionally, the color of crystals related to the dimension of the grain. However, we succeeded in obtaining RuS2 by the chemical vapor transport technique.
SampleTemperature(%) of extra Sulfure in
RuS2
Color of
Monocristal
Size   ( mm )
C S 1 1050   ° C 1 White and dull 4 × 4 × 4
C S 2 1050   ° C 2 Dull gray 4 × 4 × 3
C S 3 1025   ° C 1 Dull gray 4 × 4 × 3
C S 4 1025   ° C 2 Dull gray 4 × 3.5 × 3
C S 5 1000   ° C 1 Dull gray 3.5 × 3.5 × 3
C S 6 1000   ° C 2 Light gray 3.5 × 3 × 3
C S 7 950   ° C 1 Shiny gray 2.5 × 2 × 2
C S 8 950   ° C 2 Shiny gray 2 × 2 × 1.5
C S 9 900   ° C 1 Very Shiny gray 0.5 × 0.2 × 0.2
Table 2. Analysis of crystals formed by CVT technique.
Table 2. Analysis of crystals formed by CVT technique.
SampleTemperatureExcess of S in for RuS2Analysis of Composition
at Microprobe
Amount of Precipitate
O2
CS11050 °C1RuS1.900.005
CS21050 °C2RuS1.920.005
CS41025 °C2RuS1.94-
CS51000 °C1RuS1.95-
CS7950 °C1RuS1.96-
CS9900 °C1RuS1.97-
Table 3. Parameters of cells.
Table 3. Parameters of cells.
SampleTemperatureS2 (%) a ( Å ) ν d S - S Å d R u - s Å
CS11050 °C156350.10852.1182.369
CS31025 °C156300.10722.0972.370
CS51000 °C156240.10752.0942.367
CS61000 °C256170.10552.0522.369
CS7950 °C156110.1052.0412.368
CS9900 °C15.6090.1011.9902.373
Table 4. Exprimental parameters.
Table 4. Exprimental parameters.
SampleTemperature(%)Sa in ÅConcentration of RuSxEg Experimental (eV)
CS11050 °C15.635RuS1.901.25
CS31025 °C15.630RuS1.921.29
CS51000 °C15.624RuS1.951.36
CS61000 °C25.617RuS1.961.38
CS7950 °C15.611RuS1.961.42
CS9900 °C15.609RuS1.971.68
Table 5. Exprimental crystals paramaters.
Table 5. Exprimental crystals paramaters.
Samples d S - S ( Å ) Eg (eV) Temperature   ( ° C )
CS12.1181.251050
CS32.0971.291025
CS52.0941.361000
CS72.0411.42950
CS91.9901.68900
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Sai, R.; Gorochov, O.; Alghamdi, E.A.; Ezzaouia, H. Crystal Growth of RuS2 Using a Chemical Vapor Transport Technique and Its Properties. Crystals 2022, 12, 994. https://0-doi-org.brum.beds.ac.uk/10.3390/cryst12070994

AMA Style

Sai R, Gorochov O, Alghamdi EA, Ezzaouia H. Crystal Growth of RuS2 Using a Chemical Vapor Transport Technique and Its Properties. Crystals. 2022; 12(7):994. https://0-doi-org.brum.beds.ac.uk/10.3390/cryst12070994

Chicago/Turabian Style

Sai, Refka, Ouri Gorochov, Eman A. Alghamdi, and Hatem Ezzaouia. 2022. "Crystal Growth of RuS2 Using a Chemical Vapor Transport Technique and Its Properties" Crystals 12, no. 7: 994. https://0-doi-org.brum.beds.ac.uk/10.3390/cryst12070994

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop