Nanomodification of Lightweight Fiber Reinforced Concrete with Micro Silica and Its Influence on the Constructive Quality Coefficient

by
Evgenii M. Shcherban’
1,
Sergey A. Stel’makh
1,
Alexey Beskopylny
2,*,
Levon R. Mailyan
3,
Besarion Meskhi
4 and
Valery Varavka
5
1
Department of Engineering Geology, Bases, and Foundations, Don State Technical University, 344003 Rostov-on-Don, Russia
2
Department of Transport Systems, Faculty of Roads and Transport Systems, Don State Technical University, 344003 Rostov-on-Don, Russia
3
Department of Roads, Don State Technical University, 344003 Rostov-on-Don, Russia
4
Department of Life Safety and Environmental Protection, Faculty of Life Safety and Environmental Engineering, Don State Technical University, 344003 Rostov-on-Don, Russia
5
Research and Education Center “Materials”, Don State Technical University, Gagarin sq., 1, 344003 Rostov-on-Don, Russia
*
Author to whom correspondence should be addressed.
Submission received: 11 November 2021 / Revised: 26 November 2021 / Accepted: 28 November 2021 / Published: 30 November 2021

Abstract

:
A hypothesis was put forward that a nano-modifying additive of micro silica, which had a beneficial effect on achieving a perfect structure of heavy concrete, can also be effectively used in lightweight fiber-reinforced concrete. The nano-modifying additives of micro silica application in manufacturing lightweight fiber reinforced concrete products and structures can significantly enchain their strength characteristics without increasing their mass and consequently improve their design characteristics. The purpose of the work was to increase the structural quality coefficients for all types of strengths of lightweight fiber-reinforced concrete due to its modification with micro silica. The effect of nano-modifying additives of micro silica on the strength characteristics of lightweight fiber reinforced concrete was studied. The optimal amount of micro silica addition was experimentally confirmed and established of 10% of the cement mass. The coefficients of constructive quality for all experimentally determined strength characteristics of lightweight fiber-reinforced concrete modified with micro silica additives were calculated. The coefficient of constructive quality for tensile strength in bending of lightweight fiber reinforced concrete with additives was two and a half times higher than that of heavy concrete without additives and up to 37% higher than that of lightweight fiber-reinforced concrete without additives.

1. Introduction

Among the innovative areas that improve the efficiency of cement materials are their fine grinding, activation of water and mortars, reinforcement with fillers, etc. [1,2]. Fine grinding can be carried out in high-energy mills and rotor-pulsating units. An increase in the specific surface area of powders from 200 to 800 m2/kg leads to a significant increase in the strength of concrete. Water was activated by electric, magnetic fields, gravity, or other methods [1,2].
Considerable attention of researchers is paid to the use of production waste during new construction materials obtaining. At the same time, the following tasks are considered: environmental protection, involvement of waste in the production of building materials to reduce the consumption of cement and improve the economic performance, improving the quality of building materials, including their operational resistance and durability, creation of waste-free technologies to produce building materials. Furthermore, the structural health monitoring techniques can investigate their condition to ensure the safety of the infrastructure during its service life [3,4,5].
The finely dispersed technogenic and natural raw materials application in building manufacture is due to both factors: the need large-tonnage production wastes utilization (ash and slag mixtures, fly ash, slags, dressing waste, overburden, etc.), and the requirement to improve the quality of building materials [6,7,8]. These additives can be used to prepare binders; heavy, fine-grained, light, cellular, fire and heat-resistant, decorative and radiation-protective concretes; heat-insulating, wall, ceramic, facing, refractory products; fillers of industrial openings. In addition, mineral additives have a sealing effect on the structure of building materials, especially in multicomponent binder compositions.
The following methods can be used to increase the efficiency of cement use and reduce energy consumption in the manufacture of concrete: the inclusion of additives of micro-fillers, including micro silica and reinforcing fillers such as wollastonite; the introduction of superplasticizers; mechanical activation of cement; the impact of electromagnetic waves [9,10,11].
When non-functional organosilicon compounds and superplasticizers are used as additives, their mechanical activation is expedient. In this case, polyorganosiloxanes can enter into a chemical reaction with cement minerals, resulting in heterosiloxane structures that are resistant to the action of alkalis [12].
For example, in [13], the current state of modeling the molecular dynamics (MD) of calcium silicate hydrate (CSH) and its various modifications for nanotechnological cement composites, including carbon-based nanomaterials (for example, carbon nanotubes, graphene, graphene oxide) is comprehensively considered. It is summarized that the MD method can calculate and visualize the behavior of cement hydrates and other ingredients in a cement matrix at the nanoscale. Thus, it becomes possible to study the fundamental properties of the CSH structure and its interaction with nanoparticles [13].
Reducing the amount of clinker in cement binders is very important today, and nanotechnology allows to expand these opportunities. So, in work [14] the optimization of the binder was carried out, consisting of 60% Portland cement, 20% limestone, 20% fly ash, 3% polyvinyl alcohol (PVA) fibers, and 2% superplasticizer. Its optimization was carried out using three different nano montmorillonite (nMt) dispersions: two organically modified and one inorganic in different proportions (from 0.5% to 4%). Flexural strength, measured at 7, 28, 56 and 90 days, was improved after 28 days of hardening with the addition of inorganic nMt. Thermogravimetric analyses performed on days 7, 28, 56 and 90 combined with X-ray diffraction (on day 28) showed an enhanced pozzolanic response. Further measurements of the relative density nMt of cement nanocomposites showed higher values than that of the reference composition, which can be explained by better packing of particles. Proposals were also made for further activation of cement nanocomposites reinforced with nMt fiber. Waterproof tests have suggested that inorganic nMt may be a viable alternative material where permeability is a prerequisite [14].
The need to produce environmentally friendly cement has driven research towards nanotechnology. The main product of cement hydration—calcium silicate hydrate—is nanoscale in nature. Therefore, the addition of nanoparticles to mixed compositions of Portland cement can significantly change the mechanical strength, porosity and durability. The work [15] considers the material aspects of nanocomponents: nano-silica and montmorillonite nano clay. The disadvantages that arise when they are added to cement pastes and ways to eliminate these disadvantages were considered. It is concluded that solid particles of nano-silica in mixed cement pastes should not exceed 0.5%, and solid particles of nano clay—almost 1% of the binder mass. Finally, the authors summarize that, despite the progress made, inorganic nano clay has significant potential [15].
In [16], the effect of nano-SiO2(nS) particles on cement binders was studied. NS particles dispersed in (a) polycarboxylate or (b) water were added to a reference low carbon binder containing 43% Portland cement (PC), 20% limestone powder (LS) and 37% fly ash (FA) by weight binder. Eight quaternary binders containing nS, PC, LS and FA and eight quaternary binders containing nS, PC, LS, FA and micro silica (μS) were then tested. nS was added in an amount of 0.1%, 0.2%, 0.5% or 1.0% by weight of the binder as a substitute for LS for four-component binders and in an amount of 0.5% or 1.0% for five-component binders. It was concluded that, in such complex compositions, hydration products seem to create a shell around FA particles, delaying their activation at an early age. At a later age, the addition of 0.5% nS improved strength, microstructure and hydration. Polycarboxylate/nS particles provided a more pronounced improvement in strength with the addition of 0.5%, possibly due to their superplasticizing effect [16].
A study [17] evaluated the effect of adding nanoparticles of silicon dioxide (NS) to two binder matrices, such as ordinary Portland cement and sulfoaluminate cement, to establish their effect on mechanical and chemical properties. NS was added at doses ranging from 0.3 to 5.0% by weight concerning the cement to carry out this assessment. The results showed that the compressive strength and chemical resistance of sulfates were improved by adding silica nanoparticles to both matrices. Finally, resistance to the chemical attack of sulfates was shown to be enhanced with the addition of silicon dioxide nanoparticles compared to pure cement, indicating an increase in compaction [8].
In [18], an assessment was made of the effect of nano-silica on the calcium silicate hydrate network and the microstructure of hardened pastes based on Portland cement with ternary, quaternary and five-component systems. The sample obtained in the presence of micro silica and nano-silica (five-component combination) demonstrated the presence of a more complex gel network of calcium silicate hydrate (bridging tetrahedrons), characteristic of a honeycomb structure, in contrast to the triple combination (control sample) [18].
In the article [19], a study of the effect of nanoparticles on the mechanical properties of concrete of different ages was carried out. Various mixtures have been studied, including nano-silica (NS), nano clay (NC), or both NS and NC together with different percentages, and mechanical properties such as compressive and flexural strengths have been investigated. This study showed that nanoparticles can be very effective in improving the mechanical properties of concrete, nano-silica is more effective than nano clay in mechanical properties, and a wet mix is more effective than a dry mix. On the other hand, exceeding a certain percentage of nanoparticles in concrete negatively affects the mechanical properties. The combined use of nanoparticles (NS + NC) showed a marked improvement in the compressive strength of concrete than when using the same percentage of nanoparticles of the same type. This improvement can be explained by the reaction of nanomaterials with crystals of calcium hydroxide Ca(OH)2, which are located in the interfacial zone (ITZ) between the hardened cement paste and aggregates and form a C-SH gel and the filling action of nanoparticles, which form a more compacted microstructure. A total 3% of nanoparticles, consisting of 25% NS and 75% NC, gave the highest mechanical properties: compressive and flexural strength [19].
Polypropylene fibers with carbon nanotubes obtained by melt spinning were analyzed in [20] from the point of view of experimental mechanical properties and numerical nonlocal models. Experimental results showed that, although the applied processing conditions are such that the inclusion of carbon nanotubes does not change the crystal structure and the degree of crystallinity of the matrix-base, the tensile properties of nanocomposite fibers changed significantly depending on the filler content [20].
The effect of microstal fiber, granular light fly ash aggregate and microsilica content on the fresh and hardened properties of a high-performance binder composite (HPCC) has been experimentally investigated [21]. The mechanical and physical properties of HPCC mixtures were evaluated. The effects of fiber content, silica fume addition and artificial lightweight aggregate content were studied. The experimental results showed that the mechanical properties of the HPCC and the shrinkage characteristics improved with the increase in the volume fraction of the steel fiber. The authors summarize that the negative effect of artificial lightweight aggregate can be eliminated with silica fume [21].
Analysis of literature data [9,10,11,12,13,14,15,16,17,18,19,20,21,22,23,24,25,26,27,28,29] shows that dispersed mineral additives are widely used in the manufacture of cement building materials and products. Thus, both tasks of improving the properties of building materials and the disposal of industrial waste are being solved. At the same time, the amount of added additives in some cases is not chosen reasonably enough. The dispersion of additives, the dependence of the properties of materials based on cement on this dispersion and the amount of added additives are not always analyzed. In this regard, a study on the search for a rational formulation, dosage and interaction of micro silica with other components of heavy concrete is seen as promising.
A hypothesis was put forward that a nano-modifying additive, which has a beneficial effect on achieving a perfect structure of heavy concrete, can be simultaneously used in lightweight fiber concrete. It is assumed that the use of nano-modifying additives of micro silica in the technology of manufacturing lightweight fiber-reinforced concrete products and structures will significantly increase their strength characteristics without increasing their mass and, as a consequence, improve their design characteristics.
Scientific novelty: for the first time, studies were carried out to increase the coefficients of the constructive quality of lightweight fiber-reinforced concrete due to its modification with micro silica.
Purpose of the work: increasing the coefficients of constructive quality for all types of strengths of lightweight fiber-reinforced concrete due to its modification with micro silica. Experimental studies were carried out following the structural and methodological scheme shown in Figure 1.
After formulating the hypothesis, scientific novelty, substantiating the relevance, identifying the goal, and setting goals, we will determine the necessary set of materials, equipment, and methodological apparatus for conducting the experimental and analytical part of the study.

2. Materials and Methods

2.1. Materials

During the research, additives-free Portland cement of the PC 500 D0 brand was used, the physical and mechanical characteristics and chemical composition of which are presented in Table 1.
Granite crushed stone was used as a sizeable dense aggregate, and slag pumice was used as a porous one. The physical and mechanical characteristics of a large dense and porous aggregate are presented in Table 2 and Table 3.
Quartz sand was used as a fine aggregate, the physical characteristics of which are presented in Table 4.
For sieves with a mesh size of 2.5, 1.25, 0.63, 0.315 and 0.16, the grain size composition of the sand is given, where the upper line is the partial sieve rest, and the lower line is the full sieve rest.
Glass fiber pretreated with surfactant was used as dispersed reinforcement. Table 5 shows the physical and mechanical characteristics of the fiber used.
Micro silica grade MS-85 was used as a reaction-chemical pozzolanic additive. Table 6 shows the chemical composition of micro silica MS-85.
Polycarboxylate superplasticizer MELFLUX 5581 F manufactured by BASF Construction Additives (Krasnodar, Russia) was used as a plasticizing additive in an amount of 0.3% by weight of cement.
As a control composition, heavy concrete of class B30 was designed with the workability of the mixture corresponding to the draft of the cone 1–4 cm [30]. The content of coarse aggregate fractions is represented by the following ratio: 60–fraction 10–20 mm; 40–fraction 5–10 mm [31]. The parameters of the composition of the concrete mixture obtained as a result of calculations are reflected in Table 7.
During the manufacture of lightweight fiber-reinforced concrete, part of the volume of dense aggregate was replaced with the same volume of porous in an amount of 40%. Glass fiber was introduced in the amount of 3% by weight of the cement. The water consumption was adjusted until the required concrete mix mobility was obtained [32].

2.2. Methods

When dispersed mineral additives are introduced, their uniform distribution over the volume is very important, especially in the case of the manufacture of heavy and lightweight concretes [33,34].
The mixture of powders was processed in a homogenizer to increase the homogeneity of the binder (cement and additives).
Homogenization of Portland cement and micro silica was carried out in a planetary ball mill “Activator-4M”. General view of the planetary ball mill “Activator-4M” is shown in Figure 2, and its technical characteristics are presented in Table 8.
For the directed organization of the microstructure of the cement stone, the ratio of the diameters of the mineral additive (filler) and the binder dF/dB < l is considered favorable when the filler particles serve as a substrate onto which the products of neoplasms diffuse. In this case, diffusion is possible both through the dispersion medium and through the surface of the solvation shells. Furthermore, the outflow of the substance into the contact zone prevents the early overlap of the surface of the binder grains by nuclei, which should cause a deepening of the hydration processes.
Determination of the granulometric characteristics of powdery raw materials (Portland cement, MS) was carried out using the method of laser granulometry. This method allows to determine particles size and their percentage in the material, as well as to study their shape and morphology.
Microsizer 201C laser particle analyzer was used to carry out the particle size analysis of the mineral components. It is a fully automated device designed for fast and accurate measurement of particle size distribution in the range of 0.2–600 µm. The general view of the device is shown in Figure 3, and its technical characteristics are shown in Table 9.
The study of the microstructure was carried out on a VEGA II LMU scanning electron microscope (Tescan, Brno, Czech Republic) at an accelerating voltage of 20 kV.
Images were obtained using SE detectors. The SE (Secondary Electron) detector provides information on the surface morphology of the sample. The BSE detector (reflected or backscattered electrons) provides information about the phase and chemical inhomogeneity of the material (phases and areas with a higher average atomic weight are colored in lighter shades). The surface of the samples was sputtered with metal in an Emitech sputtering device.
The experimental research program is presented in Table 10.
Also used in this research:
technological equipment: laboratory concrete mixer BL-10 (LLC “ZZBO”, Russia, Chelyabinsk region, Zlatoust); laboratory vibrating platform SMZh-539-220A (LLC “IMASH”, Armavir, Russia);
testing equipment: hydraulic press IP-1000 (LLC NPK TEKHMASH, Neftekamsk, Republic of Bashkortostan, Russia); tensile testing machine R-50 (LLC “IMASH”, Armavir, Russia);
measuring instruments: measuring metal ruler 500 mm; laboratory scales; device for measuring deviations from the plane NPL-1; device for measuring deviations from perpendicularity NPR-1.
In the course of the study, standard test methods for raw materials and products based on them were used.
Compressive and tensile flexural strength tests were carried out by GOST 10180 “Concretes. Methods for strength determination using reference specimens” [35].
When testing for compression, sample cubes are installed with one of the selected faces on the lower base plate of the testing machine (press) centrally relative to its longitudinal axis, using the marks drawn on the plate of the testing machine.
After placing the sample on the support plates of the testing machine, align the top plate of the testing machine with the upper support face of the model so that their planes adjoin entirely one another. The sample is loaded to failure at a constant rate of load rise (0.6 ± 0.2) MPa/s.
The prism specimen is installed in the testing machine according to Figure 4 and loaded to failure at a constant rate of load growth (0.05 ± 0.01) MPa/s.
When testing for axial tension, the sample is fixed in a tensile machine and loaded to failure at a constant rate of load growth (0.05 ± 0.01) MPa/s.
The prismatic strength was determined following the requirements of GOST 24452 “Concretes. Methods of prismatic, compressive strength, modulus of elasticity and Poisson’s ratio determination” [36].
When determining the prismatic strength of concrete, loading the specimen to a load level equal to (40 ± 5)% should be performed in steps equal to 10% of the expected breaking load, keeping the loading rate (0.6 ± 0.2) MPa/s.
At each stage, load should be held for 4 to 5 min (during heating-up to 15 min) and the readings on the instruments at the beginning and at the end of the load stage should be recorded in the test log.
At a load level equal to (40 ± 5)%, remove the instruments from the sample, unless there are other requirements stipulated by the test program. After removing the devices, further loading of the sample should be carried out continuously at a constant speed in accordance with the requirements of GOST 10180-2012.
The values of the coefficients of constructive quality (CSQ) for different types of strengths were calculated using the following formulas:
C S Q R b , c u b = R b , c u b ρ
where R b , c u b is cubic compressive strength, MPa; ρ is the density of concrete, g/cm3.
C S Q R b = R b ρ
where R b is the prismatic compressive strength, MPa.
C S Q R b t b = R b t b ρ
where R b t b is tensile strength in bending, MPa.
C S Q R b t = R b t ρ
where R b t is the axial tensile strength, MPa.
Having formed the experimental-methodological apparatus and setting the parameters of the study, we present the results obtained by us in the course of our work.

3. Results

The granulometric analysis of the mineral components used—Portland cement and micro silica—is presented in Figure 5.
Based on micro silica granulometric composition shown in Figure 5, it follows that the main share (52.9%) falls on particles with a size of up to 2.58 inclusive and 47.1% for particles with the size of up to 10.27 microns. For cement (Figure 4), the maximum mass fraction (49.4%) falls on particles with a length from 17.8 to 53.7 μm, and particles with a size of up to 10 μm—24.3%. In this case, the average particle diameter of Portland cement is 31 microns, and micro silica—3.6 microns, respectively.
The results obtained from the tests of prototype cement beams with different percentages of micro silica are presented in Table 11.
From Table 10 it can be seen that the maximum values of the strength characteristics were recorded for samples of cement stone with a 10% content of silica fume additive.
As known, active mineral finely dispersed additives are capable in the presence of water interacting with portlandite— C a ( O H ) 2 at ordinary temperatures, forming compounds with astringent properties— C S H , according to the reaction scheme:
S i O 2   ( a m o r p h o u s   i n   m i n e r a l   a d d i t i v e s ) + C a ( O H ) 2 + H 2 O C S H
So, during the hydration of cement in the composition of hydrated neoplasms of cement stone, C S H and free C H are of the most significant importance of the occupied volume and effect on the properties of the cement stone. The formation of these compounds is represented by the following scheme of chemical reactions occurring during cement hydration:
C 3 S ,   C 2 S ,   C 3 A   a n d   C 4 A F + w a t e r C S H ,   C A H   a n d   C F H + C H
where C 3 S is alite ( 3 C a O x S i O 2 ) ;
C 2 S is belite ( 2 C a O x S i O 2 ) ;
C 3 A is tricalcium aluminate ( 3 C a O x A l 2 O 3 ) ;
C 4 A F is tetra calcium alumoferrite ( 4 C a O x A l 2 O 3 x F e 2 O 3 ) ;
C H is calcium hydroxide;
C S H is calcium hydrosilicates;
C A H is calcium hydroaluminates;
C F H is Calcium Hydroferrites.
Figure 6 shows a diagram of the hydration of Portland cement, which does not contain active mineral additives.
Calcium hydrosilicates are compounds that provide concrete strength. Calcium hydroxide (15–30% of the total volume of hydration products) is a substance that has a loose structure and can dissolve in water, therefore it does not play an important role in increasing the strength and durability of concrete.
Clinker hydration products with a low degree of crystallinity increase the strength of the cement stone. Therefore, to increase the density of cement stone, it is necessary to create such a structure that contains many fine-crystalline “internal products” C S H by reducing the proportion of larger-crystalline “external products” C S H (see Figure 7).
The addition of silica fume binds free C H into less soluble and denser compounds, which makes it possible to reduce the thickness and increase the density of the transition zone in concrete. Therefore, due to this pozzolanic reaction, the content of free C a ( O H ) 2 in the form of large crystals of portlandite decreases, while the content of C S H increases, increasing the strength and durability of concrete by increasing the density and strength of both the cement stone itself and the contact zone between cement stone and aggregate grains in the structure of high-strength concrete.
Using the method of electron microscopy, a comparative analysis of the effect of micro silica and a complex of micro silica (MS) + superplasticizer (SP) on the formation of the structure and properties of cement stone was carried out. Pictures of the main compositions are shown in Figure 8, Figure 9, Figure 10 and Figure 11—(a) with 2000× magnification, and (b) with 1000× magnification.
Thus, the study of cement stone chips in an electron microscope made it possible to draw the following conclusions:
-
the structure of non-additive cement stone is heterogeneous, has a block character and is represented by weakly crystallized interlayers of highly basic calcium hydrosilicates, including portlandite accumulations;
-
the addition of MS contributes to the formation of a denser homogeneous structure, preferably from low-basic calcium hydrosilicates;
-
the joint introduction of MS and SP is accompanied by the formation of a dense structure, represented by both a weakly crystallized and a gel-like phase, in which portlandite is practically not detected.
The results obtained from the tests of prototypes of lightweight fiber-reinforced concrete with different percentages of micro silica are presented in Table 12 and Figure 12.
After analyzing the obtained experimental data on the effect of the percentage of micro silica additive on the strength characteristics of lightweight fiber-reinforced concrete, the following was established:
-
the maximum germination of cubic strength is observed in the prototypes of lightweight fiber-reinforced concrete with a micro silica content of 10% (MS = 10%); so in comparison with samples of lightweight fiber-reinforced concrete without additives, it was 35%; a similar comparison was made for other compositions: so the increase for samples with MS = 6% was 17%, for samples with MS = 8–23%, for samples with MS = 12–25%;
-
the increase in prismatic compressive strength for specimens with MS = 6% was 16%, for specimens with MS = 8–25%, for specimens with MS = 10–35%, and for specimens with MS = 12–26%;
-
the increase in tensile strength in bending for specimens with MS = 6% was 12%, for specimens with MS = 8–17%, for specimens with MS = 10–37%, and for specimens with MS = 12–24 %;
-
the increase in axial tensile strength for specimens with MS = 6% was 8%, for specimens with MS = 8–16%, for specimens with MS = 10–24%, and for specimens with MS = 12–10%.
Figure 12 shows that the maximum values of the structural quality factors, calculated for various types of strength, are observed in lightweight fiber-reinforced concrete with MS = 10%.
So, in comparison with heavy concrete, the increase was:
C S Q R b , c u b : 6%;
C S Q R b : 7%;
C S Q R b t b : 253%;
C S Q R b t : 60%.
In comparison with lightweight concrete without MK-85 additive, the increase was:
- C S Q R b , c u b : 34%;
- C S Q R b : 35%;
- C S Q R b t b : 37%;
- C S Q R b t : 24%.
The coefficient of constructive quality (CSQ) for tensile strength in bending for lightweight fiber-reinforced concrete with MS = 10% is two and a half times higher than that for heavy concrete without additives due to the complex influence of the following factors:
(1)
the addition of fiber, which significantly increases the tensile strength in bending.
(2)
replacement of a part of the dense aggregate with a porous one, which leads to a significant reduction in the mass of concrete products with a slight loss of strength;
(3)
replacing part of the cement with lighter micro silica.
After carrying out experimental studies, processing the results obtained and performing the necessary calculations, as well as after completing the theoretical interpretation with the help of high-precision microscopic equipment of the physical picture of the processes of structure formation, a thorough analysis and comparison of the results obtained with the results of other authors should be carried out.

4. Discussion

The analysis of the results obtained showed the high efficiency of the proposed recipe, technological and design solutions. From the formulation point of view, the possibility of nanomodification of lightweight fiber-reinforced concrete with micro silica was established, as a result of which, firstly, the expediency of such nanomodification, and secondly, the dosage of the content of nano-modifying additives of micro silica in such concrete was determined to obtain the highest characteristics.
From a technological point of view, the compatibility of low-density dispersion-reinforced concrete with a nano-modifying additive of micro silica was tested. The revealed possibility of simple technological mixing of such components and the test results proved that the joint work of fiber-reinforcing fiber and hardening micro silica is beneficial to the resulting concrete and gives a synergistic effect.
From a constructive point of view, the possibility of dispersed reinforcement of such lightweight fiber-reinforced concrete, which, in turn, at the level of a cement stone, is nano-modified with the addition of micro silica, was determined.
This is how you can describe the qualitative picture of the study.
From a quantitative point of view, it was revealed that the optimal value of the percentage of nano-modifying additives of micro silica will be a value equal to 10%.
At the same time, the mechanism of interaction between the nano-modifying additive and the structure of the forming concrete has been studied. A high packing density of particles in such concrete was proved, and the addition of micro silica contributed to better hydration of the cement stone, its more perfect structure, and a decrease in pore space. Such an additive influenced the pore structure at the micro level, while an important factor was the simultaneous dispersed reinforcement of concrete, which ultimately turned out to be light in weight and at the same time possessing significant strength compared to analogs. In order to identify operational prospects, it was also necessary to evaluate the effectiveness of the proposed recipe, technological and design solutions not in terms of absolute indicators, but in terms of relative ones, in terms of the coefficient of constructive quality. Their effectiveness was proved due to the fact that the coefficient of constructive quality increased due to a significant increase in strength, while the mass of structures practically did not change from the introduction of a nano-modifying additive.
To assess the effectiveness of the developed proposals, it is important to conduct a comparative analysis with the results previously obtained by other authors. As already noted in the Introduction section, various authors [9,10,11,12,13,14,15,16,17,18,19,20,21,22,23,24,25,26,27,28,29] considered the issues of nanomodification of heavy concrete with various additives. We, for the first time, carried out a study of the possibility of using a nano-modifying additive, namely micro silica for dispersed reinforced concretes, among other things, having a light weight. For the first time, we studied the effect of a combination of factors of nanomodification of the structure of a cement stone, which implies the work of the additive at the micro level, and at the macro level—dispersed reinforcement with fibers. Thus, by hardening concrete at the micro and macro levels, we get a result that is different from the results of the authors who previously worked on this issue.
The novelty of the research is the application of such a combined modification of concrete at the micro and macro levels, and thus the research is original, different from the previously performed works.
For the first time, we obtained new fundamental knowledge about the formation of the microstructure of fiber-reinforced concrete with a lightweight of nanomodified micro silica additive and developed ideas about the joint work of nanomodified cement stone with dispersed fiber in lightweight fiber-reinforced concrete with an increased coefficient of structural quality.

5. Conclusions

According to the results of the literature review and analysis of sources devoted to research carried out on the topics of nano-modified concretes, it was revealed that studies aimed at increasing the coefficients of the constructive quality of lightweight fiber-reinforced concrete due to its modification with micro silica were not carried out earlier.
The effect of nano-modifying additives of micro silica on the strength characteristics of lightweight fiber-reinforced concrete was theoretically and experimentally established. Thus, the introduction of micro silica additive into Portland cement, having an average grain size of 3.6 μm, in an amount of 10% of the cement mass in combination with a superplasticizer, is the most effective. This effect of the additive is due to the fact that it acts, as it were, as a substrate for the crystallization of hydrated neoplasms.
Large-scale experimental studies were carried out, compositions were selected, new samples of materials obtained for the first time were molded.
It is proposed to evaluate the effectiveness of each accepted recipe-technological solution in terms of relative indicators—the calculated values of the structural quality coefficients for all experimentally determined strength characteristics of lightweight fiber-reinforced concrete modified with the addition of micro silica. The coefficient of constructive quality for tensile strength in bending of lightweight fiber-reinforced concrete with MK = 10% is two and a half times higher than that of heavy concrete without additives and up to 37% higher than that of lightweight fiber-reinforced concrete without additives.
The results obtained are recommended for practical application in construction and design, and are also the basis for further scientific fundamental and applied research.

Author Contributions

Conceptualization, L.R.M., S.A.S., E.M.S., A.B. and V.V.; methodology, S.A.S., E.M.S.; software, S.A.S., E.M.S., A.B. and V.V.; validation, L.R.M., S.A.S., E.M.S. and A.B.; formal analysis, S.A.S., E.M.S.; investigation, L.R.M., S.A.S., E.M.S., A.B. and B.M.; resources, B.M., V.V.; data curation, S.A.S., E.M.S.; writing—original draft preparation, S.A.S., E.M.S. and A.B.; writing—review and editing, S.A.S., E.M.S. and A.B.; visualization, S.A.S., E.M.S., A.B. and V.V.; supervision, L.R.M., B.M.; project administration, L.R.M., B.M.; funding acquisition, A.B., B.M. All authors have read and agreed to the published version of the manuscript.

Funding

The APC was funded by Don State Technical University.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The study did not report any data.

Acknowledgments

The authors would like to acknowledge the administration of Don State Technical University for their resources and financial support.

Conflicts of Interest

The authors declare no conflict of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript, or in the decision to publish the results.

References

  1. Samadi, M.; Shah, K.W.; Huseien, G.F.; Lim, N.H.A.S. Influence of Glass Silica Waste Nano Powder on the Mechanical and Microstructure Properties of Alkali-Activated Mortars. Nanomaterials 2020, 10, 324. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  2. Stel’makh, S.A.; Shcherban’, E.M.; Beskopylny, A.N.; Mailyan, L.R.; Meskhi, B.; Butko, D.; Smolyanichenko, A.S. Influence of Composition and Technological Factors on Variatropic Efficiency and Constructive Quality Coefficients of Lightweight Vibro-Centrifuged Concrete with Alkalized Mixing Water. Appl. Sci. 2021, 11, 9293. [Google Scholar] [CrossRef]
  3. Bekzhanova, Z.; Memon, S.A.; Kim, J.R. Self-Sensing Cementitious Composites: Review and Perspective. Nanomaterials 2021, 11, 2355. [Google Scholar] [CrossRef]
  4. Lyapin, A.; Beskopylny, A.; Meskhi, B. Structural Monitoring of Underground Structures in Multi-Layer Media by Dynamic Methods. Sensors 2020, 20, 5241. [Google Scholar] [CrossRef] [PubMed]
  5. Beskopylny, A.; Lyapin, A.; Kadomtsev, M.; Veremeenko, A. Complex method of defects diagnostics in underground structures. MATEC Web Conf. 2018, 146, 02013. [Google Scholar] [CrossRef] [Green Version]
  6. Luo, J.; Chen, S.; Li, Q.; Liu, C.; Gao, S.; Zhang, J.; Guo, J. Influence of Graphene Oxide on the Mechanical Properties, Fracture Toughness, and Microhardness of Recycled Concrete. Nanomaterials 2019, 9, 325. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  7. Zhang, P.; Sha, D.; Li, Q.; Zhao, S.; Ling, Y. Effect of Nano Silica Particles on Impact Resistance and Durability of Concrete Containing Coal Fly Ash. Nanomaterials 2021, 11, 1296. [Google Scholar] [CrossRef]
  8. Chu, H.; Zhang, Y.; Wang, F.; Feng, T.; Wang, L.; Wang, D. Effect of Graphene Oxide on Mechanical Properties and Durability of Ultra-High-Performance Concrete Prepared from Recycled Sand. Nanomaterials 2020, 10, 1718. [Google Scholar] [CrossRef] [PubMed]
  9. Rassokhin, A.S.; Ponomarev, A.N.; Figovsky, O.L. Silica fumes of different types for high-performance fine-grained concrete. Mag. Civ. Eng. 2018, 78, 151–160. [Google Scholar] [CrossRef]
  10. Klyuev, S.V.; Klyuev, A.V.; Abakarov, A.D.; Shorstova, E.S.; Gafarova, N.G. The effect of particulate reinforcement on strength and deformation characteristics of fine-grained concrete. Mag. Civ. Eng. 2017, 75, 66–75. [Google Scholar] [CrossRef]
  11. Bily, P.; Fladr, J.; Chylik, R.; Vrablik, L.; Hrbek, V. The effect of cement replacement and homogenization procedure on concrete mechanical properties. Mag. Civ. Eng. 2019, 86, 46–60. [Google Scholar] [CrossRef]
  12. Vavrenyuk, S.V.; Efimenko, Y.V.; Vavrenyuk, V.G. Mechanical Activation, Mineral Powders, Chemical Modification, Solid-Phase Reactivity, Polyorganosiloxanes. IOP Conf. Ser. Mater. Sci. Eng. 2021, 1079, 072043. [Google Scholar] [CrossRef]
  13. Cho, B.H.; Chung, W.; Nam, B.H. Molecular Dynamics Simulation of Calcium-Silicate-Hydrate for Nano-Engineered Cement Composites—A Review. Nanomaterials 2020, 10, 2158. [Google Scholar] [CrossRef]
  14. Papatzani, S.; Grammatikos, S.; Paine, K. Permeable Nanomontmorillonite and Fibre Reinforced Cementitious Binders. Materials 2019, 12, 3245. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  15. Papatzani, S. Effect of nanosilica and montmorillonite nanoclay particles on cement hydration and microstructure. Mater. Sci. Technol. 2016, 32, 138–153. [Google Scholar] [CrossRef]
  16. Papatzani, S.; Paine, K. Optimization of low carbon footprint quaternary and quinary (37% fly ash) cementitious nanocomposites with polycarboxylate or aqueous nanosilica particles. Adv. Mater. Sci. Eng. 2019, 2019, 5931306. [Google Scholar] [CrossRef] [Green Version]
  17. Gómez-Zamorano, L.Y.; Castillo-Linton, C.E. Effect of the addition of nanosilica particles on the properties of two cementitious matrices. Revista ALCONPAT 2016, 6, 101–115. [Google Scholar] [CrossRef] [Green Version]
  18. Calabria-Holley, J.; Paine, K.; Papatzani, S. Effects of nanosilica on the calcium silicate hydrates in Portland cement–fly ash systems. Adv. Cem. Res. 2015, 27, 187–200. [Google Scholar] [CrossRef] [Green Version]
  19. Mohamed, A.M. Influence of nano materials on flexural behavior and compressive strength of concrete. HBRC J. 2016, 12, 212–225. [Google Scholar] [CrossRef] [Green Version]
  20. Acierno, S.; Barretta, R.; Luciano, R.; Marotti de Sciarra, F.; Russo, P. Experimental evaluations and modeling of the tensile behavior of polypropylene/single-walled carbon nanotubes fibers. Compos. Struct. 2017, 174, 12–18. [Google Scholar] [CrossRef]
  21. Mermerdaş, K.; İpek, S.; Algın, Z.; Ekmen, Ş.; Güneş, İ. Combined effects of microsilica, steel fibre and artificial lightweight aggregate on the shrinkage and mechanical performance of high strength cementitious composite. Construct. Build. Mater. 2020, 262, 120048. [Google Scholar] [CrossRef]
  22. Ferrotto, M.F.; Fischer, O.; Cavaleri, L. Analysis-oriented stress–strain model of CRFP-confined circular concrete columns with applied preload. Mater. Struct. 2018, 51, 44. [Google Scholar] [CrossRef]
  23. Horňáková, M.; Lehner, P. Relationship of Surface and Bulk Resistivity in the Case of Mechanically Damaged Fibre Reinforced Red Ceramic Waste Aggregate Concrete. Materials 2020, 13, 5501. [Google Scholar] [CrossRef]
  24. Hameed, M.A.S.; Maula, B.H.; Bahnam, Q.M. An empirical relationship between compressive strength and ultrasonic pulse velocity for concrete. Int. Rev. Civ. Eng. 2019, 10. [Google Scholar] [CrossRef]
  25. Kim, J.-J.; Yoo, D.-Y. Effects of fiber shape and distance on the pullout behavior of steel fibers embedded in ultra-high-performance concrete. Cem. Concr. Compos. 2019, 103, 213–223. [Google Scholar] [CrossRef]
  26. Belyaev, A.V.; Nesvetaev, G.V.; Mailyan, D.R. Design features of three-layer slab reinforced concrete structures. Mater. Sci. Forum 2018, 931, 264–268. [Google Scholar] [CrossRef]
  27. Shilov, A.; Polskoy, P.; Mailyan, D.; Shilov, P. Initial crack effect on the strength of oblique cross sections of reinforced concrete beams strengthened with carbon fiber. E3S Web Conf. 2019, 110, 01053. [Google Scholar] [CrossRef]
  28. Polskoy, P.P.; Mailyan, D.R.; Shilov, A.A. The cut span effect on the beams inclined sections strength reinforced with external composite reinforcement. Mater. Sci. Forum 2020, 974, 633–637. [Google Scholar] [CrossRef]
  29. Beskopylny, A.; Lyapin, A.; Anysz, H.; Meskhi, B.; Veremeenko, A.; Mozgovoy, A. Artificial neural networks in classification of steel grades based on non-destructive tests. Materials 2020, 13, 2445. [Google Scholar] [CrossRef] [PubMed]
  30. GOST 10181 Concrete Mixtures. Methods of Testing. Available online: https://docs.cntd.ru/document/1200115733 (accessed on 28 November 2021).
  31. Mailyan, L.R.; Beskopylny, A.N.; Meskhi, B.; Shilov, A.V.; Stel’makh, S.A.; Shcherban’, E.M.; Smolyanichenko, A.S.; El’shaeva, D. Improving the Structural Characteristics of Heavy Concrete by Combined Disperse Reinforcement. Appl. Sci. 2021, 11, 6031. [Google Scholar] [CrossRef]
  32. Mailyan, L.R.; Beskopylny, A.N.; Meskhi, B.; Stel’makh, S.A.; Shcherban, E.M.; Ananova, O. Optimization of Composition and Technological Factors for the Lightweight Fiber-Reinforced Concrete Production on a Combined Aggregate with an Increased Coefficient of Structural Quality. Appl. Sci. 2021, 11, 7284. [Google Scholar] [CrossRef]
  33. Shcherban, E.M.; Prokopov, A.Y.; Stelmakh, S.A.; Shuyskiy, A.I. Effect of Disperse Reinforcement on the Structural Quality Factor of Vibrated and Centrifuged Concretes on the Combined Aggregate. Mater. Sci. Forum 2020, 974, 283–287. [Google Scholar] [CrossRef]
  34. Stelmakh, S.A.; Shuyskiy, A.I.; Shcherban, E.M.; Prokopov, A.Y. Efficiency Comparison of Fiber Reinforcement in Vibrated and Centrifuged Concretes at Different Types of the Applied Heavy Aggregate. Mater. Sci. Forum 2019, 974, 288–292. [Google Scholar] [CrossRef]
  35. GOST 10180 Concretes. Methods for Strength Determination Using Reference Specimens. Available online: http://docs.cntd.ru/document/1200100908 (accessed on 28 November 2021).
  36. GOST 24452 Concretes. Methods of Prismatic, Compressive Strength, Modulus of Elasticity and Poisson’s Ratio Determination. Available online: https://docs.cntd.ru/document/9056198 (accessed on 28 November 2021).
Figure 1. Structural and methodological scheme of experimental research.
Figure 1. Structural and methodological scheme of experimental research.
Materials 14 07347 g001
Figure 2. Planetary mill “Activator-4M”.
Figure 2. Planetary mill “Activator-4M”.
Materials 14 07347 g002
Figure 3. Laser particle analyzer Microsizer 201C.
Figure 3. Laser particle analyzer Microsizer 201C.
Materials 14 07347 g003
Figure 4. Flexural tensile test setup (a—width and height of the sample; F—load; q—distributed load; l—span; 1—sample; 2—articulated fixed support; 3—articulated-movable support).
Figure 4. Flexural tensile test setup (a—width and height of the sample; F—load; q—distributed load; l—span; 1—sample; 2—articulated fixed support; 3—articulated-movable support).
Materials 14 07347 g004
Figure 5. Particle size distribution of (a) Portland cement, (b) micro silica particles.
Figure 5. Particle size distribution of (a) Portland cement, (b) micro silica particles.
Materials 14 07347 g005
Figure 6. Hydration of Portland cement in the absence of micro silica addition (A—Portland cement; B—water; C— C S H ; D— C H ).
Figure 6. Hydration of Portland cement in the absence of micro silica addition (A—Portland cement; B—water; C— C S H ; D— C H ).
Materials 14 07347 g006
Figure 7. Development of the microstructure of cement stone in the process of hydration of Portland cement, where: Fss—calcium aluminoferrite; AFt—calcium hydrosulfoaluminate; AFm—calcium hydrosulfoaluminoferrite.
Figure 7. Development of the microstructure of cement stone in the process of hydration of Portland cement, where: Fss—calcium aluminoferrite; AFt—calcium hydrosulfoaluminate; AFm—calcium hydrosulfoaluminoferrite.
Materials 14 07347 g007
Figure 8. Photo of the microstructure of a cement stone without additives: (a) with 2000× magnification (b) with 1000× magnification.
Figure 8. Photo of the microstructure of a cement stone without additives: (a) with 2000× magnification (b) with 1000× magnification.
Materials 14 07347 g008
Figure 9. Photo of the microstructure of a cement stone with an MS-85 additive in an amount of 6%: (a) with 2000× magnification (b) with 1000× magnification.
Figure 9. Photo of the microstructure of a cement stone with an MS-85 additive in an amount of 6%: (a) with 2000× magnification (b) with 1000× magnification.
Materials 14 07347 g009
Figure 10. Photo of the microstructure of a cement stone with an MS-85 additive in an amount of 10% and an additive of MELFLUX 5581 superplasticizer: (a) with 2000× magnification (b) with 1000× magnification.
Figure 10. Photo of the microstructure of a cement stone with an MS-85 additive in an amount of 10% and an additive of MELFLUX 5581 superplasticizer: (a) with 2000× magnification (b) with 1000× magnification.
Materials 14 07347 g010
Figure 11. Photo of the microstructure of a cement stone containing an MS-85 additive in an amount of 12% and an additive of MELFLUX 5581 superplasticizer: (a) with 2000× magnification (b) with 1000× magnification.
Figure 11. Photo of the microstructure of a cement stone containing an MS-85 additive in an amount of 12% and an additive of MELFLUX 5581 superplasticizer: (a) with 2000× magnification (b) with 1000× magnification.
Materials 14 07347 g011
Figure 12. Values of structural quality factors for various types of concrete (HC—heavy concrete; LFC—lightweight fiber concrete; LFC-6—lightweight fiber concrete with MS = 6%; LFC-8—with MS = 8%; LFC-10—with MS = 10%; LFC-12—with MS = 12%).
Figure 12. Values of structural quality factors for various types of concrete (HC—heavy concrete; LFC—lightweight fiber concrete; LFC-6—lightweight fiber concrete with MS = 6%; LFC-8—with MS = 8%; LFC-10—with MS = 10%; LFC-12—with MS = 12%).
Materials 14 07347 g012
Table 1. Physical and mechanical characteristics of Portland cement PC 500 D0 and its chemical composition.
Table 1. Physical and mechanical characteristics of Portland cement PC 500 D0 and its chemical composition.
Indicator TitleValue
Physics and Mechanics
Compressive strength at the age of 28 days, MPa54.8
Setting time, min
-start
-the end

155
220
Fineness of grinding, passage through a sieve No. 008, %96.7
Specific surface, m2/kg331
Normal density of cement paste, %23.5
Chemical
Weight loss on ignition, %0.70
Silicon oxide content (SiO2), %20.89
Aluminum oxide content (Al2O3), %4.72
Iron oxide content, (Fe2O3), %4.32
Calcium oxide content (CaO), %63.27
Magnesium oxide (MgO), wt %2.45
Sulfuric acid anhydride (SO3), wt %2.81
Alkaline oxides in terms of Na2O, wt %0.69
Free calcium oxide content (CaOfr), %0.00
Chloride ion (Cl), wt %0.038
Insoluble residue, %0.20
Table 2. Physical and mechanical characteristics of crushed granite.
Table 2. Physical and mechanical characteristics of crushed granite.
FractionBulk Density, kg/m3True Density, kg/m3Crushing, wt %Content of Lamellar and Needle-Shaped Grains, wt %Voidness, %
5–201437262011.48.145
Table 3. Physical and mechanical characteristics of slag pumice.
Table 3. Physical and mechanical characteristics of slag pumice.
FractionBulk Density, kg/m3True Density, kg/m3Strength by
GOST 32496-2013, MPa
Voidness, %
5–2061213100.853
Table 4. Physical characteristics of dense fine aggregate.
Table 4. Physical characteristics of dense fine aggregate.
Grain CompositionPassing through a Sieve No 0.16, wt. %Fineness ModulusContent of Dust and Clay Particles, %True Density, g/cm3Bulk Density, kg/m3
Sieve Size, mm
Partial and Full Sieve Rest, %
1052.51.250.630.3150.16
000.171.398.8645.8041.032.491.661.126501438
0.171.5610.4256.2197.2599.74
Table 5. Physical and mechanical properties of fiber.
Table 5. Physical and mechanical properties of fiber.
Glass FiberTensile Strength, MPaFiber Diameter, μmFiber Length, mmElastic Modulus, GPaDensity, kg/m3Elongation to Break,%
310013127226004.6
Table 6. Chemical composition of micro silica MS-85.
Table 6. Chemical composition of micro silica MS-85.
MaterialOxide Content, %
SiO2Al2O3Fe2O3CaOMgOR2OSO3Loss on Ignition
МК-8582.31.73.01.10.20.83.57.4
Table 7. Parameters of the composition of the concrete mixture.
Table 7. Parameters of the composition of the concrete mixture.
Indicator TitleW/CPC, kg/m3W, l/m3CS, kg/m3S, kg/m3ρcm, kg/m3
Indicator value0.5832719013155732405
Note: W/PC—water-cement ratio, W—water consumption, CS—crushed stone consumption, S—sand consumption, ρcm—concrete mix density.
Table 8. Technical characteristics of “Activator-4M”.
Table 8. Technical characteristics of “Activator-4M”.
Indicator TitleUnitsValue
Planetary disc:
-rotational speed
-effective diameter

rpm
mm

100–800
400
Rotation speed of drumsrpm150–1650
Centrifugal accelerationm/s21500
Drumspieces4
Drum volumemL1000
Loading ballsg600–1400
Powder loadingg50–400
Steel grade (balls) ShH15SG
Drums sizesmmØ95 × 180
Table 9. Technical characteristics of Microsizer 201C.
Table 9. Technical characteristics of Microsizer 201C.
Indicator TitleUnitsValue
Particle size rangeμm0.2–600
Radiation source He-Ne laser
Detector Photodiode Array
Number of registration channelspieces38
Sample preparation system Ultrasonic Disperser
Sample chamber volumeml50
Ultrasonic frequencykHz50
Ultrasonic powerWUp to 200
Table 10. Experimental research program.
Table 10. Experimental research program.
Research TypeSamples Number
Investigation of the microstructure of a cement stone modified with micro silicaCement beam without additives, size 40 × 40 × 160 mm–3 pcs.
Cement beam with MS-85 additive in the amount of 6%, size 40 × 40 × 160 mm–3 pcs.
Cement beam with MS-85 additive in 10% and addition of MELFLUX 5581 superplasticizer, size 40 × 40 × 160 mm–3 pcs.
Investigation of the properties (density and strength) of lightweight concrete with MS-85 additivesA total of 6 series of samples were made: heavy concrete; lightweight fiber-reinforced concrete without adding MS-85; lightweight fiber-reinforced concrete with MS-85 additive in the amount of 6%; lightweight fiber-reinforced concrete with MS-85 additive in the amount of 8%; lightweight fiber-reinforced concrete with MS-85 additive in the amount of 10%; lightweight fiber-reinforced concrete with MS-85 additive in the amount of 12%. Each series of samples contains: cubes 100 × 100 × 100–3 pcs; prisms with dimensions 100 × 100 × 400 mm–9 pcs.
Table 11. Results of tests for strength in compression and tensile in bending of cement bar specimens with different MS content.
Table 11. Results of tests for strength in compression and tensile in bending of cement bar specimens with different MS content.
CompositionCompressive Strength, MPaTensile Strength in Bending, MPa
C55.36.4
C + 6% MS-8559.87.1
C + 10% MS-85 + SP64.77.8
C + 12% MS-85 + SP61.37.4
Table 12. Test results of prototypes of heavy concrete and lightweight fiber-reinforced concrete with different percentages of micro silica.
Table 12. Test results of prototypes of heavy concrete and lightweight fiber-reinforced concrete with different percentages of micro silica.
Concrete CharacteristicsHeavy ConcreteLightweight Fiber Concrete
МS-85 Content, wt % by Cement Mass
0681012
Density, kg/m3241420872097208920952091
Cubic compressive strength, MPa63.843.751.253.758.954.7
Prismatic compressive strength, MPa47.232.337.540.343.840.6
Flexural tensile strength, MPa7.712.313.814.416.915.3
Axial tensile strength, MPa4.55.05.45.86.25.5
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Shcherban’, E.M.; Stel’makh, S.A.; Beskopylny, A.; Mailyan, L.R.; Meskhi, B.; Varavka, V. Nanomodification of Lightweight Fiber Reinforced Concrete with Micro Silica and Its Influence on the Constructive Quality Coefficient. Materials 2021, 14, 7347. https://0-doi-org.brum.beds.ac.uk/10.3390/ma14237347

AMA Style

Shcherban’ EM, Stel’makh SA, Beskopylny A, Mailyan LR, Meskhi B, Varavka V. Nanomodification of Lightweight Fiber Reinforced Concrete with Micro Silica and Its Influence on the Constructive Quality Coefficient. Materials. 2021; 14(23):7347. https://0-doi-org.brum.beds.ac.uk/10.3390/ma14237347

Chicago/Turabian Style

Shcherban’, Evgenii M., Sergey A. Stel’makh, Alexey Beskopylny, Levon R. Mailyan, Besarion Meskhi, and Valery Varavka. 2021. "Nanomodification of Lightweight Fiber Reinforced Concrete with Micro Silica and Its Influence on the Constructive Quality Coefficient" Materials 14, no. 23: 7347. https://0-doi-org.brum.beds.ac.uk/10.3390/ma14237347

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop